Palladium-silver doped carbonized Raney copper catalyst and preparation method thereof and method for preparing 1-butene by selective hydrogenation of C4 raffinate
Through the palladium-silver-doped Rainie copper carbonized catalyst, the problem of unsatisfactory activity and high reactor ratio of the existing carbon tetraselective hydrogenation catalyst is solved, and efficient 1-butene preparation is achieved, reducing costs and maintaining for a long time. catalytic activity.
Patent Information
- Application Number
- CN202111261296.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-28
AI Technical Summary
The catalytic activity of the existing carbon four-selective hydrogenation catalyst is not ideal, and the reactor ratio is high, resulting in low usage efficiency and high cost.
Using palladium-silver doped Rainey copper catalyst, the copper powder, aluminum powder, silver powder, palladium powder and other raw materials are molded and calcined, forming a copper-aluminum-palladium-silver multi-component alloy, and extracting aluminum with caustic aqueous solution , a catalyst with high catalytic activity and stability is formed.
It effectively reduces the stack ratio of the catalyst, improves the utilization rate of active components, reduces the cost of use, and maintains good activity during long-term reactions, thereby improving the selectivity and conversion of 1-butene.
Smart Images

Figure BDA0003325830450000121 
Figure BDA0003325830450000122 
Figure BDA0003325830450000123
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of C4 raffinate hydrogenation, and in particular to a palladium-silver doped carbonized Raney copper catalyst and a preparation method thereof, and a method for preparing 1-butene by selective hydrogenation of C4 raffinate. Background Art
[0002] The petroleum hydrocarbon steam cracking ethylene unit produces a large amount of mixed C4 by-products, of which 1,3-butadiene accounts for about 50% by mass. Usually, this part of 1,3-butadiene is extracted from C4 by extraction and other methods. The remaining fraction after extraction is called C4 raffinate, which contains a small amount of 1,3-butadiene, and the 1,3-butadiene needs to be hydrogenated to 1-butene.
[0003] At present, the catalyst used for the selective hydrogenation of C4 to butene is usually prepared by an impregnation method, in which an alumina carrier is impregnated in an active metal salt solution or an organic metal compound solution, and then the impregnation product is roasted and finally reduced to obtain an alumina-supported catalyst. Due to the use of the impregnation method, the dispersion of the active components in the catalyst is low, which in turn affects the full play of the catalytic performance. More importantly, during the high-temperature roasting process, the active components sinter, resulting in a decrease in the performance of the catalyst, which significantly affects the butadiene conversion rate and 1-butene selectivity of the C4 selective hydrogenation reaction.
[0004] Raney copper catalysts are highly active and can achieve better reaction results than traditional alumina-based catalysts. However, in practical applications, due to their high density and large stacking ratio, the effective utilization rate of the active components of the Raney copper catalyst is low, which affects its efficiency and results in higher usage costs. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of unsatisfactory catalytic activity and high bulk density of the prior art C4 selective hydrogenation catalyst for preparing butene, and to provide a palladium-silver doped carbided Raney copper catalyst and a preparation method thereof, and a method for preparing 1-butene by selective hydrogenation of C4 raffinate.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a palladium-silver doped Raney copper carbide catalyst, comprising:
[0007] (1) mixing a carbonizable organic matter, a curing agent, and a curing accelerator to obtain a mixture;
[0008] (2) forming copper powder, aluminum powder, silver powder, palladium powder, a binder, nitric acid and the mixed material to obtain a catalyst precursor;
[0009] (3) calcining the catalyst precursor to obtain a calcined product;
[0010] (4) The calcined product is treated with a caustic soda aqueous solution to extract aluminum to obtain a palladium-silver doped Raney copper carbide catalyst.
[0011] The second aspect of the present invention provides a palladium-silver doped Raney copper carbide catalyst prepared by the method described in the first aspect.
[0012] The third aspect of the present invention provides a method for preparing 1-butene by selective hydrogenation of C4 raffinate, comprising: contacting the C4 raffinate with a catalyst for hydrogenation reaction to obtain 1-butene; wherein the C4 raffinate contains 1,3-butadiene; the catalyst is the palladium-silver doped carbide Raney copper catalyst described in the second aspect;
[0013] The conditions of the hydrogenation reaction include: a molar ratio of hydrogen to 1,3-butadiene of (0.2-10):1, a reactor inlet temperature of 30-60°C, a reaction pressure of 0.5-3MPa, and a reaction space velocity of 2-20h / min based on the liquid volume of C4 raffinate. -1 .
[0014] Through the above technical solution, the method provided by the present invention has the following beneficial effects:
[0015] (1) forming a copper-aluminum-palladium-silver multi-component alloy by calcining the metal raw materials, wherein the interaction between the metals contained in the alloy is more obvious, and the aluminum, silver and palladium can effectively disperse the copper particles, thereby avoiding the aggregation of active components;
[0016] (2) The introduction of carbon carrier can effectively reduce the bulk ratio of the catalyst. Compared with the ordinary Raney copper catalyst using pure alloy blocks, the bulk ratio can be reduced by about one-fourth, thereby improving the utilization rate of the active components in the catalyst and reducing the cost of the catalyst.
[0017] (3) The catalyst provided by the present invention has better stability and is used for the selective hydrogenation of C4 raffinate to prepare 1-butene. The catalyst still maintains good activity after the reaction is carried out for 100 hours. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0020] The first aspect of the present invention provides a method for preparing a palladium-silver doped carbonized Raney copper catalyst, comprising:
[0021] (1) mixing a carbonizable organic matter, a curing agent, and a curing accelerator to obtain a mixture;
[0022] (2) forming copper powder, aluminum powder, silver powder, palladium powder, a binder, nitric acid and the mixed material to obtain a catalyst precursor;
[0023] (3) calcining the catalyst precursor to obtain a calcined product;
[0024] (4) The calcined product is treated with a caustic soda aqueous solution to extract aluminum to obtain a palladium-silver doped Raney copper carbide catalyst.
[0025] According to the present invention, in step (1), the carbonizable organic matter, the curing agent and the curing accelerator are mixed to obtain a mixture, namely, a curing system. The curing system can be a liquid system, a powder system or a granular system.
[0026] In the present invention, the carbonizable organic matter refers to the organic matter that is treated under certain temperature and atmosphere conditions, and the hydrogen, oxygen, nitrogen, sulfur, etc. in the organic matter are fully or partially volatilized, thereby obtaining a synthetic material with a high carbon content, and the obtained carbon material has the properties of high temperature resistance, high strength, high modulus, porosity, etc. Preferably, the carbonizable organic matter can be an organic polymer compound, and more preferably at least one of epoxy resin, phenolic resin, furan resin, polystyrene, starch and lignin.
[0027] In the present invention, preferably, the curing agent may be selected from at least one of methyltetrahydrophthalic anhydride, hexamethylenetetramine and polyaniline.
[0028] In the present invention, preferably, the curing agent accelerator may be selected from at least one of triethanolamine, polythiophene and polypyrrole.
[0029] According to the present invention, in step (1), preferably, the weight ratio of the carbonizable organic matter: curing agent: curing accelerator can be (40-60): (40-60): (0.1-2), and more preferably (50-60): (40-50): (0.1-1).
[0030] According to the present invention, in step (2), the binder can promote the bonding of the raw material components to facilitate the molding process, and can also play a dispersing role, which helps to obtain the catalyst precursor with uniform distribution of components after the molding process. Preferably, the binder can be selected from at least one of pseudo-boehmite, soluble starch, carboxymethyl cellulose and polyethylene glycol, and is more preferably pseudo-boehmite.
[0031] According to the present invention, in step (2), the nitric acid may be a dilute nitric acid aqueous solution. Preferably, the concentration of the nitric acid may be 1-10 wt %.
[0032] According to the present invention, in step (2), preferably, the weight ratio of the binder to nitric acid can be 1:(0.5-1.5), and more preferably 1:(1-1.2).
[0033] According to the present invention, in step (2), preferably, the weight ratio of copper powder: aluminum powder: silver powder: palladium powder: binder: the mixture can be (20-40): (20-40): (0.1-5): (0.01-0.2): (10-30): (10-25), and further preferably (25-35): (25-35): (0.2-2): (0.01-0.1): (10-30): (15-25), so that the obtained palladium-silver doped Raney copper carbide catalyst has higher catalytic activity and stability.
[0034] According to the present invention, in step (2), the present invention has no particular limitation on the molding process, and conventional processes in the art may be used, including but not limited to extrusion molding, sheeting molding, rolling molding, etc.
[0035] According to the present invention, in step (3), the calcination is carried out under an inert atmosphere to carbonize the organic matter to form a carbon carrier, and the inert protective gas used can be an inert gas such as nitrogen, helium, argon, etc. Preferably, the calcination conditions may include: a temperature of 600-1000°C and a time of 1-10h;
[0036] Further preferably, the calcination conditions may include: a temperature of 600-800° C. and a time of 6-8 h.
[0037] According to the present invention, in step (4), the aluminum extraction treatment is mainly used to extract part of the aluminum in the calcined product alloy. In particular, when the binder is pseudo-boehmite, it is used as a component of the catalyst precursor, and is converted into aluminum oxide after calcination and dispersed in the calcined product alloy. During the aluminum extraction treatment, the above-mentioned part of the aluminum oxide in the calcined product alloy can also be dissolved to form pores, thereby making the prepared palladium-silver-doped Raney copper carbide catalyst have higher catalytic activity and catalyst utilization. Preferably, the caustic alkali can use sodium hydroxide and / or potassium hydroxide, and sodium hydroxide is more preferably used.
[0038] According to the present invention, in step (4), the caustic soda is mixed with water to form a caustic soda aqueous solution when used. Preferably, the concentration of the caustic soda aqueous solution can be 2-40wt%, and more preferably 5-20wt%, so that the prepared palladium-silver doped Raney copper carbide catalyst has higher catalytic activity.
[0039] According to the present invention, in step (4), in order to make the surface of the prepared palladium-silver-doped Raney copper carbide catalyst have a sufficient amount of active copper components to obtain higher catalytic activity, preferably, the weight ratio of the calcined product: caustic soda can be 1: (1-3), and more preferably 1: (1-2).
[0040] According to the present invention, in step (4), preferably, the conditions for the aluminum extraction treatment may include: a temperature of 20-100° C. and a time of 0.5-2 h;
[0041] Further preferably, the conditions for the aluminum extraction treatment may include: a temperature of 50-90° C. and a time of 1-2 hours, so that the prepared palladium-silver doped Raney copper carbide catalyst has higher catalytic activity and stability.
[0042] According to the present invention, step (4) further comprises washing the palladium-silver-doped Raney copper carbide catalyst obtained by the aluminum extraction treatment with deionized water until the pH value of the washing liquid is 7-9, and then storing the catalyst product in deionized water or anhydrous ethanol for use. Preferably, the temperature of the deionized water used for washing can be 20-40° C., and the pH value of the washing liquid is 7-8.
[0043] According to the present invention, the method further comprises the following steps before the molding process: copper powder, aluminum powder, silver powder and palladium powder are mixed, and then the mixture, binder and nitric acid are added for kneading to obtain a plastic body. The present invention has no particular limitation on the mixing and kneading, and the mixing and kneading can be carried out by conventional methods and equipment in the art. Preferably, for example, copper powder, aluminum powder, silver powder and palladium powder can be placed in a kneader to be fully stirred and mixed, and then the mixture, binder and nitric acid are added for kneading to obtain a uniform plastic body, and then the plastic body is subjected to molding treatment.
[0044] The second aspect of the present invention provides a palladium-silver doped Raney copper carbide catalyst prepared by the method described in the first aspect.
[0045] According to the present invention, preferably, based on the total weight of the palladium-silver doped Raney copper carbide catalyst, in the catalyst, the content of silver is 0.5-2 wt %, and the content of palladium is 0.02-0.1 wt %.
[0046] The third aspect of the present invention provides a method for preparing 1-butene by selective hydrogenation of C4 raffinate, comprising: contacting the C4 raffinate with a catalyst for hydrogenation reaction to obtain 1-butene; wherein the C4 raffinate contains 1,3-butadiene; the catalyst is the palladium-silver doped carbide Raney copper catalyst described in the second aspect;
[0047] The conditions of the hydrogenation reaction include: a molar ratio of hydrogen to 1,3-butadiene of (0.2-10):1, a reactor inlet temperature of 30-60°C, a reaction pressure of 0.5-3MPa, and a reaction space velocity of 2-20h / min based on the liquid volume of C4 raffinate. -1 .
[0048] According to the present invention, further preferably, the conditions of the hydrogenation reaction may include: a molar ratio of hydrogen to 1,3-butadiene of (0.5-5):1, a reactor inlet temperature of 40-60°C, a reaction pressure of 1.5-3 MPa, and a reaction space velocity of 10-20 h / min based on the liquid volume of the C4 raffinate. -1 .
[0049] The present invention will be described in detail below by way of examples. In the following examples and comparative examples,
[0050] The contents of silver and palladium in the catalyst were measured by X-ray fluorescence spectrometry (XRF).
[0051] Unless otherwise specified, all raw materials used are common commercially available products.
[0052] Example 1
[0053] (1) stirring a liquid epoxy resin, methyltetrahydrophthalic anhydride and triethanolamine to fully mix them to obtain a mixture;
[0054] Wherein, the weight ratio of liquid epoxy resin: methyltetrahydrophthalic anhydride: triethanolamine is 100:85:1.5;
[0055] (2) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding the mixture prepared in step (1), pseudo-boehmite and a 2 wt% dilute nitric acid aqueous solution, kneading them thoroughly to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0056] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite: mixed material is 125: 125: 3: 0.2: 80: 80; the weight ratio of pseudo-boehmite: nitric acid is 1: 1.1;
[0057] (3) placing the catalyst precursor obtained in step (2) in a tubular high-temperature electric furnace, passing nitrogen protection, and calcining at 650° C. for 6 hours, and cooling under nitrogen protection to obtain a calcined product;
[0058] (4) The calcined product obtained in step (3) is placed in a 20 wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product to the solute NaOH is 1:1; the conditions for the aluminum extraction are: temperature 85°C, time 1 h), and the obtained palladium-silver-doped Raney copper carbide catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0059] The prepared palladium-silver doped Raney copper carbide catalyst was recorded as C1. XRF detection showed that the silver content in C1 was 1 wt %, and the palladium content was 0.06 wt %.
[0060] Example 2
[0061] (1) stirring a liquid epoxy resin, methyltetrahydrophthalic anhydride and triethanolamine to fully mix them to obtain a mixture;
[0062] The weight ratio of liquid epoxy resin: methyltetrahydrophthalic anhydride: triethanolamine is 100: 85: 1.5;
[0063] (2) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding the mixture prepared in step (1), pseudo-boehmite and a 2 wt% dilute nitric acid aqueous solution, kneading them thoroughly to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0064] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite: mixed material is 125: 125: 3.5: 0.2: 100: 80; the weight ratio of pseudo-boehmite: nitric acid is 1: 1.2;
[0065] (3) placing the catalyst precursor obtained in step (2) in a tubular high-temperature electric furnace, passing nitrogen protection, and calcining at 600° C. for 6 hours, and cooling under nitrogen protection to obtain a calcined product;
[0066] (4) The calcined product obtained in step (3) is placed in a 20wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:2; the conditions for the aluminum extraction treatment are: temperature 80°C, time 1h), and the obtained palladium-silver-doped Raney copper carbide catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0067] The prepared palladium-silver doped Raney copper carbide catalyst was recorded as C2. XRF detection showed that the silver content in C2 was 1.2 wt %, and the palladium content was 0.05 wt %.
[0068] Example 3
[0069] (1) stirring a liquid epoxy resin, methyltetrahydrophthalic anhydride and triethanolamine to fully mix them to obtain a mixture;
[0070] Wherein, the weight ratio of liquid epoxy resin: methyltetrahydrophthalic anhydride: triethanolamine is 100:85:1.5;
[0071] (2) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding the mixture prepared in step (1), pseudo-boehmite and a 2 wt% dilute nitric acid aqueous solution, kneading them thoroughly to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0072] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite: mixed material is 125: 125: 3.5: 0.4: 50: 80; the weight ratio of pseudo-boehmite: nitric acid is 1: 1.1;
[0073] (3) placing the catalyst precursor obtained in step (2) in a tubular high-temperature electric furnace, passing nitrogen protection, and calcining at 650° C. for 8 h, and cooling under nitrogen protection to obtain a calcined product;
[0074] (4) The calcined product obtained in step (3) is placed in a 20wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:2; the conditions for the aluminum extraction treatment are: temperature 90°C, time 1h), and the obtained palladium-silver-doped Raney copper carbide catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0075] The prepared palladium-silver doped Raney copper carbide catalyst was recorded as C3. XRF detection showed that the silver content in C3 was 1.3 wt %, and the palladium content was 0.08 wt %.
[0076] Example 4
[0077] (1) stirring phenolic resin, hexamethylenetetramine and triethanolamine to fully mix them to obtain a mixture;
[0078] The weight ratio of phenolic resin: hexamethylenetetramine: triethanolamine is 100:80:1.5;
[0079] (2) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding the mixture prepared in step (1), pseudo-boehmite and a 2 wt% dilute nitric acid aqueous solution, kneading them thoroughly to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0080] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite: mixed material is 125: 125: 3.5: 0.2: 120: 80; the weight ratio of pseudo-boehmite: nitric acid is 1: 1.2;
[0081] (3) placing the catalyst precursor obtained in step (2) in a tubular high-temperature electric furnace, passing nitrogen protection, and calcining at 700° C. for 6 hours, and cooling under nitrogen protection to obtain a calcined product;
[0082] (4) The calcined product obtained in step (3) is placed in a 20wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:2; the conditions for the aluminum extraction treatment are: temperature 80°C, time 1h), and the obtained palladium-silver-doped Raney copper carbide catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0083] The prepared palladium-silver doped Raney copper carbide catalyst was recorded as C4. XRF detection showed that the silver content in C4 was 1 wt %, and the palladium content was 0.05 wt %.
[0084] Example 5
[0085] (1) stirring phenolic resin, hexamethylenetetramine and triethanolamine to fully mix them to obtain a mixture;
[0086] Wherein, the weight ratio of phenolic resin: hexamethylenetetramine: triethanolamine is 100:80:1.5;
[0087] (2) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding the mixture prepared in step (1), pseudo-boehmite and a 2 wt% dilute nitric acid aqueous solution, kneading them thoroughly to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0088] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite: mixed material is 125: 125: 3.5: 0.2: 150: 80; the weight ratio of pseudo-boehmite: nitric acid is 1: 1.05;
[0089] (3) placing the catalyst precursor obtained in step (2) in a tubular high-temperature electric furnace, passing nitrogen protection, and calcining at 650° C. for 6 hours, and cooling under nitrogen protection to obtain a calcined product;
[0090] (4) The calcined product obtained in step (3) is placed in a 20 wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:2; the conditions for the aluminum extraction treatment are: temperature 85°C, time 1 h), and the obtained palladium-silver-doped Raney copper carbide catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0091] The prepared palladium-silver doped Raney copper carbide catalyst was recorded as C5. XRF detection showed that the silver content in C5 was 0.7 wt %, and the palladium content was 0.03 wt %.
[0092] Comparative Example 1
[0093] The method of Example 1 is followed, except that palladium powder is not used in step (2), that is, the weight ratio of copper powder: aluminum powder: silver powder: pseudo-boehmite: mixed material in the raw materials is 125:125:3:80:80, and other conditions are the same as those of Example 1. The prepared silver-doped supported Raney copper catalyst is denoted as D1.
[0094] XRF analysis revealed that the silver content in D1 was 1 wt%.
[0095] Comparative Example 2
[0096] (1) Weigh 200 g of copper-aluminum alloy block (alloy block of about 0.9-3.2 mm obtained by crushing copper-aluminum alloy) and slowly add it into a 20 wt% sodium hydroxide solution (the mass of the solute NaOH is 200 g) in batches for activation for 2 h. The copper-aluminum alloy treated as above is washed with deionized water at 40° C. until the washing liquid is neutral;
[0097] (2) Weigh 15.6 g of silver nitrate and place it in a 100 mL volumetric flask and dilute to volume with water to obtain a silver nitrate solution with a silver content of 100 mg / mL;
[0098] (3) 30 mL of the copper-aluminum alloy obtained in step (1) was added to 50 mL of deionized water, and 10 mL of the silver nitrate solution obtained in step (2) was added. The mixture was reacted for 2 h and then filtered. The obtained catalyst was recorded as D2.
[0099] XRF analysis revealed that the silver content in D3 was 1.38 wt%.
[0100] Comparative Example 3
[0101] Weigh 100 g of an alumina carrier (average particle size: 3.5 mm), and spray 70 mL of a mixed aqueous solution of palladium nitrate and silver nitrate (wherein the silver content is 20 mg / mL and the palladium content is 1 mg / mL) onto the alumina carrier. After drying, place the carrier in an oven at 120°C for 24 h. The dried product is calcined at 450°C for 8 h to decompose the nitrate, and then reduced by purging with hydrogen at 150°C for 2 h. The resulting catalyst is recorded as D4.
[0102] XRF detection showed that the silver content in D4 was 1.4wt%, and the palladium content was 0.08wt%.
[0103] Comparative Example 4
[0104] The catalyst prepared according to the method and parameter conditions of Example 10 in CN107952450A is denoted as D4.
[0105] XRF detection showed that the silver content in D4 was 0.73wt%, and the palladium content was 0.12wt%.
[0106] Test Case
[0107] The catalysts C1-C5 and D1-D4 prepared in Examples 1-5 and Comparative Examples 1-4 were used in the test of selective hydrogenation of C4 raffinate to produce 1-butene, to evaluate the catalytic activity and stability of the catalysts. The test process is as follows:
[0108] 45 mL of catalyst was loaded into the fixed bed reactor, and after nitrogen replacement, the C4 raffinate (composition shown in Table 1) was mixed with hydrogen and then introduced into the reactor. The reaction conditions were: the molar ratio of hydrogen to 1,3-butadiene was 1.2:1, the reactor inlet temperature was 50°C, the reaction pressure was 2.3 MPa, and the reaction space velocity measured by the liquid volume of the C4 raffinate was 20 h -1 .
[0109] After the reaction was carried out for 10 h and 100 h, the contents of 1,3-butadiene at the reactor inlet and outlet and the content of 1-butene at the outlet were measured, and the conversion rate and selectivity of 1,3-butadiene hydrogenation to 1-butene were calculated. The results are shown in Table 2. The calculation formula is as follows:
[0110]
[0111]
[0112] Table 1
[0113] Components Content / wt% Components Content / wt% Isobutane 1.86 1,2-Butadiene 0.004 n-Butane 14.32 1,3-Butadiene 1.92 trans-2-butene 18.33 Ethyl acetylene 0.024 1-Butene 16.52 Vinyl Acetylene 0.006 Isobutylene 35.87 Methylacetylene - Cis-2-Butene 11.06
[0114] Table 2
[0115]
[0116]
[0117] Note: In Table 2, the numbers before Ag and Pd represent their percentage content in the catalyst. For example, the catalyst composition 1Ag-0.06Pd-Raney Cu / C of C1 means that based on the total weight of catalyst C1, the contents of Ag and Pd in the catalyst are 1% and 0.06%, respectively.
[0118] As can be seen from Table 2, the palladium-silver doped carbonized Raney copper catalysts C1-C5 provided by the present invention have high 1,3-butadiene conversion rate and 1-butene selectivity in the reaction of selective hydrogenation of C4 raffinate to prepare 1-butene. Compared with the initial stage of the reaction, the decrease in the above two indicators is smaller after the reaction is carried out for 100 hours, which indicates that the palladium-silver doped supported Raney copper catalyst provided by the present invention has good catalytic activity and stability.
[0119] In particular, in Comparative Example 1, no metal palladium was used, and only metal silver was used for single doping, and the performance of the obtained catalyst could not reach the effect of C1-C5; in Comparative Example 2, since the silver nitrate solution was unstable and easily hydrolyzed, silver was easily aggregated on the carrier surface, resulting in a significant difference in the catalytic activity and stability of D2 compared with C1-C5; the dispersion of the active metal in the catalyst D3 of Comparative Example 3 was uncontrollable, and the acidity of alumina caused the catalyst to be unstable, which further affected the hydrogenation activity and stability; in Comparative Example 4, although carbonization was also used in the catalyst preparation process, the doping of silver and palladium was doped on the surface of the alloy by surface replacement reaction, resulting in a difference in the catalytic activity and stability of D4 compared with C1-C5.
[0120] In addition, the present invention can effectively reduce the stacking ratio of the catalyst by introducing a carbon carrier. Compared with ordinary Raney copper catalysts, the utilization rate of active components is higher, which can reduce the use cost of the catalyst.
[0121] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a palladium-silver doped Raney copper carbide catalyst, It is characterized in that include: (1) mixing a carbonizable organic matter, a curing agent, and a curing accelerator to obtain a mixture; (2) forming copper powder, aluminum powder, silver powder, palladium powder, a binder, nitric acid and the mixed material to obtain a catalyst precursor; (3) calcining the catalyst precursor to obtain a calcined product; (4) extracting aluminum from the calcined product with a caustic soda aqueous solution to obtain a palladium-silver doped Raney copper carbide catalyst; Wherein, in step (2), the weight ratio of copper powder:aluminum powder:silver powder:palladium powder:binder:the mixture is (20-40):(20-40):(0.1-5):(0.01-0.2):(10-30):(10-25).
2. The method according to claim 1, in, The carbonizable organic matter is an organic macromolecular compound; And / or, the curing agent is selected from at least one of methyltetrahydrophthalic anhydride, hexamethylenetetramine and polyaniline; and / or, the curing agent accelerator is selected from at least one of triethanolamine, polypyrrole and polythiophene; And / or, the binder is selected from at least one of pseudo-boehmite, soluble starch, carboxymethyl cellulose and polyethylene glycol; And / or, the concentration of the nitric acid is 1-10wt%.
3. The method according to claim 2, in, The carbonizable organic matter is at least one of epoxy resin, phenolic resin, furan resin, polystyrene, starch and lignin; And / or, the binder is pseudo-boehmite.
4. The method according to any one of claims 1 to 3, in, In step (1), the weight ratio of the carbonizable organic matter: curing agent: curing accelerator is (40-60): (40-60): (0.1-2).
5. The method according to claim 4, in, In step (1), the weight ratio of the carbonizable organic matter: curing agent: curing accelerator is (50-60): (40-50): (0.1-1).
6. The method according to any one of claims 1 to 3, in, In step (2), the weight ratio of copper powder: aluminum powder: silver powder: palladium powder: binder: the mixed material is (25-35): (25-35): (0.2-2): (0.01-0.1): (10-30): (15-25); And / or, the weight ratio of the binder: nitric acid is 1: (0.5-1.5).
7. The method according to claim 6, in, In step (2), the weight ratio of the binder to nitric acid is 1:(1-1.2).
8. The method according to any one of claims 1 to 3, in, In step (3), the calcination conditions include: temperature of 600-1000° C.; time of 1-10 h.
9. The method according to claim 8, in, In step (3), the calcination conditions include: temperature of 600-800°C; time of 5-8h.
10. The method according to claim 9, in, The calcination is performed under an inert atmosphere.
11. The method according to any one of claims 1 to 3, in, In step (4), the caustic alkali is sodium hydroxide and / or potassium hydroxide; And / or, the concentration of the caustic alkali aqueous solution is 2-40wt%.
12. The method according to claim 11, in, In step (4), the caustic soda is sodium hydroxide; And / or, the concentration of the caustic alkali aqueous solution is 5-20wt%.
13. The method according to claim 12, in, In step (4), the weight ratio of the calcined product to the caustic soda is 1:(1-3); And / or, the conditions for the aluminum extraction process include: a temperature of 20-100° C.; and a time of 0.5-2 h.
14. The method according to claim 13, in, In step (4), the weight ratio of the calcined product to the caustic soda is 1:(1-2); And / or, the conditions for the aluminum extraction treatment include: temperature of 50-90° C.; time of 1-2 h.
15. The method according to any one of claims 1 to 3, in, The method further comprises, before the molding process, performing the following steps: Copper powder, aluminum powder, silver powder and palladium powder are mixed, and then the mixture, a binder and nitric acid are added and kneaded to obtain a plastic body.
16. A palladium-silver doped Raney copper carbide catalyst prepared by the method according to any one of claims 1 to 15.
17. A method for preparing 1-butene by selective hydrogenation of C4 raffinate, It is characterized in that include: The C4 raffinate is contacted with a catalyst for hydrogenation reaction to obtain 1-butene; wherein the C4 raffinate contains 1,3-butadiene; the catalyst is the palladium-silver doped carbided Raney copper catalyst as claimed in claim 16; The conditions of the hydrogenation reaction include: the molar ratio of hydrogen to 1,3-butadiene is (0.2-10):1, the reactor inlet temperature is 30-60°C, the reaction pressure is 0.5-3MPa, and the reaction space velocity measured by the liquid volume of C4 raffinate is 2-20h -1 .