Palladium-silver doped Raney copper catalyst and preparation method thereof and method for preparing 1-butene by selective hydrogenation of C4 raffinate
Through the palladium-silver doped Rainie copper catalyst, the copper-aluminum-palladium-silver alloy is formed by calcining and extraction of aluminum, which solves the problem of unsatisfactory activity and stability of the existing catalysts, and significantly improves the carbon quad-extraction residue 1- Conversion and selectivity of butene.
Patent Information
- Application Number
- CN202111261560.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-28
AI Technical Summary
The catalytic activity and stability of the existing carbon tetra-selective hydrogenation catalysts are not ideal, which affects the conversion rate and product selectivity of 1-butene in the carbon tetra-selective residue.
Using the Rainie copper catalyst doped with palladium silver, it is calcined and extracted by molding copper powder, aluminum powder, silver powder and binder to form a copper aluminum palladium silver multi-component alloy to improve metal dispersion and catalyst activity and the use of specific binders and caustics to form pores to enhance the stability of the catalyst.
The activity and stability of the catalyst are improved, the conversion rate and selectivity of 1-butene in the carbon quadruple extraction residue are enhanced, and the activity remains good after 100 hours of reaction is maintained, which significantly improves the catalytic performance.
Smart Images

Figure BDA0003325930390000101 
Figure BDA0003325930390000102 
Figure BDA0003325930390000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of C4 raffinate hydrogenation, and in particular to a palladium-silver doped Raney copper catalyst and a preparation method thereof, and a method for preparing 1-butene by selective hydrogenation of C4 raffinate. Background Art
[0002] In the method of producing butene by cracking C4, one route is to first separate the 1,3-butadiene in the cracked C4. The remaining by-product mainly containing C4 alkanes and C4 monoolefins is called C4 raffinate. The C4 raffinate contains a trace amount of 1,3-butadiene, accounting for about 1% by weight, which will have a great impact on subsequent chemical utilization such as etherification reaction and alkylation reaction. Therefore, it must be removed by selective hydrogenation.
[0003] The catalysts currently used in industry for selective hydrogenation of C4 to butene include Pd / Al 2 O 3 Catalyst, also Pd-Ag / Al 2 O 3 The catalysts are all supported catalysts, and the preparation method adopted is the traditional impregnation method. The dispersion of the catalysts obtained by this method is often low, which affects the full play of the catalytic performance of the active components, resulting in the activity and stability of the catalysts being less than ideal.
[0004] Therefore, the development of catalysts with higher catalytic activity and stability is of great significance for improving the conversion rate and product selectivity of 1-butene by selective hydrogenation of C4 raffinate. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem of unsatisfactory catalytic activity and stability of the prior art C4 selective hydrogenation catalyst for preparing butene, and to provide a palladium-silver doped Raney copper catalyst and a preparation method thereof, and a method for preparing 1-butene by selective hydrogenation of C4 raffinate.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a palladium-silver doped Raney copper catalyst, comprising:
[0007] (1) subjecting copper powder, aluminum powder, silver powder, palladium powder, a binder and nitric acid to a molding process to obtain a catalyst precursor;
[0008] (2) calcining the catalyst precursor to obtain a calcined product;
[0009] (3) The calcined product is treated with a caustic soda aqueous solution to extract aluminum to obtain a palladium-silver doped Raney copper catalyst.
[0010] The second aspect of the present invention provides a palladium-silver doped Raney copper catalyst prepared by the method described in the first aspect.
[0011] The third aspect of the present invention provides a method for preparing 1-butene by selective hydrogenation of C4 raffinate, comprising: contacting the C4 raffinate with a catalyst for hydrogenation reaction to obtain 1-butene; wherein the C4 raffinate contains 1,3-butadiene; the catalyst is the palladium-silver doped Raney copper catalyst described in the second aspect;
[0012] The conditions of the hydrogenation reaction include: a molar ratio of hydrogen to 1,3-butadiene of (0.2-10):1, a reactor inlet temperature of 30-60°C, a reaction pressure of 0.5-3MPa, and a reaction space velocity of 2-20h / min based on the liquid volume of C4 raffinate. -1 .
[0013] Through the above technical solution, the method provided by the present invention has the following beneficial effects:
[0014] (1) forming a copper-aluminum-palladium-silver multi-component alloy by calcining the metal raw materials, wherein the interaction between the metals contained in the alloy is more obvious, and the aluminum, silver and palladium can effectively disperse the copper particles, thereby avoiding the aggregation of active components;
[0015] (2) The introduction of a specific binder effectively reduces the catalyst stacking ratio, and while extracting aluminum from the alloy, the caustic soda partially corrodes the aluminum oxide from the binder, thereby forming channels in the catalyst, which helps the reactants enter the catalyst for reaction, thereby improving the catalyst activity and utilization rate;
[0016] (3) In the Raney copper catalyst doped with single metal silver, the doping process of surface silver is a replacement reaction, which will lead to the reduction of active metal copper and the decrease of catalyst activity. The calcination method is used to prepare an alloy containing silver and palladium, which can solve the problem of the decrease of active metal copper leading to the decrease of catalyst activity and improve the stability of the catalyst. The catalyst provided by the present invention is used for the selective hydrogenation of C4 raffinate to prepare 1-butene, and the reaction still maintains good activity after 100 hours. DETAILED DESCRIPTION
[0017] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0019] The first aspect of the present invention provides a method for preparing a palladium-silver doped Raney copper catalyst, comprising:
[0020] (1) subjecting copper powder, aluminum powder, silver powder, palladium powder, a binder and nitric acid to a molding process to obtain a catalyst precursor;
[0021] (2) calcining the catalyst precursor to obtain a calcined product;
[0022] (3) The calcined product is treated with a caustic soda aqueous solution to extract aluminum to obtain a palladium-silver doped Raney copper catalyst.
[0023] According to the present invention, in step (1), the binder can promote the bonding of the raw material components to facilitate the molding process, and can also play a dispersing role, which helps to obtain the catalyst precursor with uniform distribution of components after the molding process. Preferably, the binder can be selected from at least one of pseudo-boehmite, soluble starch, carboxymethyl cellulose and polyethylene glycol, and is more preferably pseudo-boehmite.
[0024] According to the present invention, in step (1), the nitric acid may be a dilute nitric acid aqueous solution, and preferably, the concentration of the nitric acid is 1-10 wt %.
[0025] According to the present invention, in step (1), in order to make the prepared palladium-silver doped Raney copper catalyst have higher catalytic activity and stability, preferably, the weight ratio of the copper powder: aluminum powder: silver powder: palladium powder: binder can be (30-45): (30-45): (0.1-5): (0.01-0.2): (10-40), and more preferably (35-42): (35-45): (0.2-2): (0.01-0.1): (16-30); preferably, the weight ratio of the binder: nitric acid can be: 1: (0.5-1.5), and more preferably 1: (1-1.2).
[0026] According to the present invention, in step (1), the present invention has no particular limitation on the molding process, and conventional processes in the art may be used, including but not limited to extrusion molding, sheet molding, rolling molding, etc.
[0027] According to the present invention, in step (2), the catalyst precursor can be calcined in a conventional sintering device in the art, such as a tube furnace or a muffle furnace. The calcination has no special requirements on the atmosphere and can be carried out in an air atmosphere or an inert atmosphere. Preferably, the calcination conditions may include: a temperature of 600-1000°C and a time of 1-10h;
[0028] Further preferably, the calcination conditions may include: a temperature of 600-800° C. and a time of 5-8 h.
[0029] According to the present invention, in step (3), the aluminum extraction treatment is mainly used to extract part of the aluminum in the calcined product alloy. In particular, when the binder is pseudo-boehmite, it is a component of the catalyst precursor, which is converted into aluminum oxide after calcination and dispersed in the calcined product alloy. During the aluminum extraction treatment, the above-mentioned part of the aluminum oxide in the calcined product alloy can also be dissolved, so that pores are formed in the catalyst, which can further improve the catalyst activity and utilization rate. Preferably, the caustic alkali can use sodium hydroxide and / or potassium hydroxide, and sodium hydroxide is more preferably used.
[0030] According to the present invention, in step (3), the caustic soda is mixed with water to form a caustic soda aqueous solution. Preferably, the concentration of the caustic soda aqueous solution can be 2-40wt%, more preferably 10-30wt%, so that the prepared palladium-silver doped Raney copper catalyst has higher catalytic activity.
[0031] According to the present invention, in step (3), preferably, the weight ratio of the calcined product: caustic soda can be 1: (1-3), and more preferably 1: (1-2), so that the surface of the prepared palladium-silver-doped Raney copper catalyst has a sufficient amount of active copper components to obtain higher catalytic activity.
[0032] According to the present invention, in step (3), preferably, the conditions for the aluminum extraction treatment may include: a temperature of 20-100° C. and a time of 0.5-2 h;
[0033] Further preferably, the conditions for the aluminum extraction treatment may include: a temperature of 50-90° C. and a time of 1-2 hours, so that the prepared palladium-silver doped Raney copper catalyst has higher catalytic activity and stability.
[0034] According to the present invention, step (3) further comprises washing the palladium-silver-doped Raney copper catalyst obtained by the aluminum extraction treatment with deionized water until the pH value of the washing liquid is 7-9, and then storing the catalyst product in deionized water or anhydrous ethanol for use. Preferably, the temperature of the deionized water used for washing can be 20-40° C., and the pH value of the washing liquid is 7-8.
[0035] According to the present invention, the method further comprises the following steps before the molding process: copper powder, aluminum powder, silver powder and palladium powder are mixed, and then a binder and nitric acid are added for kneading to obtain a plastic body. The present invention has no particular limitation on the mixing and kneading, and the mixing and kneading can be carried out by conventional methods and equipment in the art. Preferably, for example, copper powder, aluminum powder, silver powder and palladium powder can be placed in a kneader to be fully stirred and mixed, and then a binder and nitric acid are added for kneading to obtain a uniform plastic body, and then the plastic body is subjected to molding treatment.
[0036] The second aspect of the present invention provides a palladium-silver doped Raney copper catalyst prepared by the method described in the first aspect.
[0037] According to the present invention, preferably, based on the total weight of the palladium-silver doped Raney copper catalyst, in the catalyst, the content of silver is 0.5-2 wt %, and the content of palladium is 0.02-0.1 wt %.
[0038] The third aspect of the present invention provides a method for preparing 1-butene by selective hydrogenation of C4 raffinate, comprising: contacting the C4 raffinate with a catalyst for hydrogenation reaction to obtain 1-butene; wherein the C4 raffinate contains 1,3-butadiene; the catalyst is the palladium-silver doped Raney copper catalyst described in the second aspect;
[0039] The conditions of the hydrogenation reaction may include: a molar ratio of hydrogen to 1,3-butadiene of (0.2-10): 1, a reactor inlet temperature of 30-60°C, a reaction pressure of 0.5-3MPa, and a reaction space velocity of 2-20h / min based on the liquid volume of C4 raffinate. -1 .
[0040] According to the present invention, further preferably, the conditions of the hydrogenation reaction may include: a molar ratio of hydrogen to 1,3-butadiene of (0.5-5):1, a reactor inlet temperature of 40-60°C, a reaction pressure of 1.5-3 MPa, and a reaction space velocity of 10-20 h / min based on the liquid volume of the C4 raffinate. -1 .
[0041] The present invention will be described in detail below by way of examples. In the following examples and comparative examples,
[0042] The contents of silver and palladium in the catalyst were measured by X-ray fluorescence spectrometry (XRF).
[0043] Unless otherwise specified, all raw materials used are commercially available.
[0044] Example 1
[0045] (1) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding pseudo-boehmite and a 2 wt% diluted nitric acid aqueous solution, kneading them fully to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0046] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite is 125:125:3:0.2:80; the weight ratio of pseudo-boehmite: dilute nitric acid aqueous solution is 1:1.125;
[0047] (2) placing the catalyst precursor obtained in step (1) in a high temperature furnace and calcining at 650° C. for 6 h to obtain a calcined product;
[0048] (3) The calcined product obtained in step (2) is placed in a 20 wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:2; the conditions for the aluminum extraction treatment are: the temperature is 85°C and the time is 1 h), and the obtained palladium-silver-doped Raney copper catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0049] The prepared palladium-silver doped Raney copper catalyst was recorded as S1. XRF detection showed that the silver content in S1 was 1.2 wt %, and the palladium content was 0.08 wt %.
[0050] Example 2
[0051] (1) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding pseudo-boehmite and a 2 wt% diluted nitric acid aqueous solution, kneading them fully to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0052] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite is 125:125:3.5:0.2:100; the weight ratio of pseudo-boehmite: dilute nitric acid aqueous solution is 1:1;
[0053] (2) placing the catalyst precursor obtained in step (1) in a high-temperature furnace and calcining at 600° C. for 5 h to obtain a calcined product;
[0054] (3) The calcined product obtained in step (2) is placed in a 20 wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:1; the conditions for the aluminum extraction treatment are: temperature 90°C, time 1 h), and the obtained palladium-silver-doped Raney copper catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0055] The prepared palladium-silver doped Raney copper catalyst was recorded as S2. XRF detection showed that the silver content in S2 was 1.4 wt %, and the palladium content was 0.08 wt %.
[0056] Example 3
[0057] (1) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding pseudo-boehmite and a 2 wt% diluted nitric acid aqueous solution, kneading them fully to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0058] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite is 125:125:3.5:0.15:50; the weight ratio of pseudo-boehmite: dilute nitric acid aqueous solution is 1:1.2;
[0059] (2) placing the catalyst precursor obtained in step (1) in a high temperature furnace and calcining at 650° C. for 6 h to obtain a calcined product;
[0060] (3) The calcined product obtained in step (2) is placed in a 20 wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:2; the conditions for the aluminum extraction treatment are: the temperature is 85°C and the time is 1 h), and the obtained palladium-silver-doped Raney copper catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0061] The prepared palladium-silver doped Raney copper catalyst was recorded as S3. XRF detection showed that the silver content in S3 was 1.6 wt %, and the palladium content was 0.06 wt %.
[0062] Example 4
[0063] (1) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding pseudo-boehmite and a 2 wt% diluted nitric acid aqueous solution, kneading them fully to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0064] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite is 125:125:3.5:0.16:120; the weight ratio of pseudo-boehmite: dilute nitric acid aqueous solution is 1:1.1;
[0065] (2) placing the catalyst precursor obtained in step (1) in a high temperature furnace and calcining at 600° C. for 6 h to obtain a calcined product;
[0066] (3) The calcined product obtained in step (2) is placed in a 20wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:2; the conditions for the aluminum extraction treatment are: temperature 95°C, time 1h), and the obtained palladium-silver-doped Raney copper catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0067] The prepared palladium-silver doped Raney copper catalyst was recorded as S4. XRF detection showed that the silver content in S4 was 1.2 wt %, and the palladium content was 0.04 wt %.
[0068] Example 5
[0069] (1) adding copper powder, aluminum powder, silver powder and palladium powder into a kneader, stirring and mixing them uniformly, then adding pseudo-boehmite and a 2 wt% diluted nitric acid aqueous solution, kneading them fully to obtain a uniform plastic body, and then extruding and pelletizing to obtain a catalyst precursor;
[0070] The weight ratio of copper powder: aluminum powder: silver powder: palladium powder: pseudo-boehmite is 125:125:3.5:0.1:150; the weight ratio of pseudo-boehmite: dilute nitric acid aqueous solution is 1:1.05;
[0071] (2) placing the catalyst precursor obtained in step (1) in a high temperature furnace and calcining at 650° C. for 6 h to obtain a calcined product;
[0072] (3) The calcined product obtained in step (2) is placed in a 20wt% NaOH aqueous solution for aluminum extraction (wherein the weight ratio of the calcined product: the solute NaOH is 1:1; the conditions for the aluminum extraction treatment are: temperature 85°C, time 1h), and the obtained palladium-silver-doped Raney copper catalyst is washed with deionized water until the pH value of the washing liquid is 7-9, and then stored in deionized water or anhydrous ethanol for use.
[0073] The prepared palladium-silver doped Raney copper catalyst was recorded as S5. XRF detection showed that the silver content in S5 was 0.9 wt %, and the palladium content was 0.02 wt %.
[0074] Comparative Example 1
[0075] The method of Example 2 is followed, except that palladium powder is not used in step (1), the weight ratio of copper powder: aluminum powder: silver powder: pseudo-boehmite in the raw materials is 125:125:3.5:100; the weight ratio of pseudo-boehmite: dilute nitric acid aqueous solution is 1:1.1. Other conditions are the same as those of Example 2. The obtained catalyst is recorded as D1.
[0076] XRF analysis revealed that the silver content in D1 was 1.4 wt%.
[0077] Comparative Example 2
[0078] (1) Weigh 200 g of copper-aluminum alloy block (alloy block of about 0.9-3.2 mm obtained by crushing copper-aluminum alloy) and slowly add it into a 20 wt% sodium hydroxide solution (the mass of the solute NaOH is 200 g) in batches for activation for 2 h. The copper-aluminum alloy treated as above is washed with deionized water at 40° C. until the washing liquid is neutral;
[0079] (2) Weigh 15.6 g of silver nitrate and place it in a 100 mL volumetric flask and dilute to volume with water to obtain a silver nitrate solution with a silver content of 100 mg / mL;
[0080] (3) 30 mL of the copper-aluminum alloy obtained in step (1) was added to 50 mL of deionized water, and 10 mL of the silver nitrate solution obtained in step (2) was added. The mixture was reacted for 2 h and then filtered. The obtained catalyst was recorded as D2.
[0081] XRF detection showed that the silver content in D2 was 1.38wt%.
[0082] Comparative Example 3
[0083] Weigh 100 g of an alumina carrier (average particle size: 3.5 mm), and spray 70 mL of a mixed aqueous solution of palladium nitrate and silver nitrate (wherein the silver content is 20 mg / mL and the palladium content is 1 mg / mL) onto the alumina carrier. After drying, place the carrier in an oven at 120°C for 24 h. The dried product is calcined at 450°C for 8 h to decompose the nitrate, and then reduced by purging with hydrogen at 150°C for 2 h. The resulting catalyst is recorded as D3.
[0084] XRF detection showed that the silver content in D3 was 1.4wt%, and the palladium content was 0.08wt%.
[0085] Test Case
[0086] The catalysts S1-S5 and D1-D3 prepared in Examples 1-5 and Comparative Examples 1-3 were used in the test of selective hydrogenation of C4 raffinate to produce 1-butene, to evaluate the catalytic activity and stability of the catalysts. The test process is as follows:
[0087] 45 mL of catalyst was loaded into the fixed bed reactor, and after nitrogen replacement, the C4 raffinate (composition shown in Table 1) was mixed with hydrogen and then introduced into the reactor. The reaction conditions were: the molar ratio of hydrogen to 1,3-butadiene was 1.2:1, the reactor inlet temperature was 50°C, the reaction pressure was 2.3 MPa, and the reaction space velocity measured by the liquid volume of the C4 raffinate was 20 h -1 .
[0088] After the reaction was carried out for 10 hours and 100 hours, the contents of 1,3-butadiene at the inlet and outlet of the reactor and the content of 1-butene at the outlet were measured, and the conversion rate and selectivity of 1,3-butadiene hydrogenation to 1-butene were calculated. The results are shown in Table 2. The calculation formula is as follows:
[0089]
[0090]
[0091] Table 1
[0092] Components Content / wt% Components Content / wt% Isobutane 1.86 1,2-Butadiene 0.004 n-Butane 14.32 1,3-Butadiene 1.92 trans-2-butene 18.33 Ethyl acetylene 0.024 1-Butene 16.52 Vinyl Acetylene 0.006 Isobutylene 35.87 Methylacetylene - Cis-2-Butene 11.06
[0093] Table 2
[0094]
[0095] Note: In Table 2, the numbers before Ag and Pd represent their percentage content in the catalyst. For example, the catalyst composition of S1, 1.2Ag-0.08Pd-Raney Cu, means that based on the total weight of catalyst S1, the contents of Ag and Pd in the catalyst are 1.2% and 0.08%, respectively.
[0096] As can be seen from Table 2, the palladium-silver doped Raney copper catalysts S1-S5 provided by the present invention have higher 1,3-butadiene conversion rate and 1-butene selectivity in the reaction. Compared with the initial stage of the reaction, the decrease in the above two indicators is smaller after the reaction is carried out for 100 hours, which indicates that the palladium-silver doped Raney copper catalyst provided by the present invention has good catalytic activity and stability.
[0097] In particular, in Comparative Example 1, where no metallic palladium was used, the hydrogenation activity of the Raney copper catalyst doped with metallic silver decreased, the stability was reduced, and the performance could not reach the effect of S1-S5.
[0098] Comparative Example 2 adopts a surface loading method so that the surface silver of the catalyst occupies the site of active copper. Although Comparative Example 3 also adopts a palladium-silver doping method, it adopts a conventional impregnation method and uses alumina as a carrier to prepare the catalyst, resulting in uncontrollable dispersion of the metal on the carrier. The above factors lead to a significant gap in the comprehensive performance of catalytic activity and stability of D2 and D3 compared with S1-S5.
[0099] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a palladium-silver doped Raney copper catalyst, characterized in that: include: (1) subjecting copper powder, aluminum powder, silver powder, palladium powder, a binder and nitric acid to a molding process to obtain a catalyst precursor; The binder is pseudo-boehmite; (2) calcining the catalyst precursor to obtain a calcined product; (3) extracting aluminum from the calcined product with a caustic soda aqueous solution to obtain a palladium-silver doped Raney copper catalyst; The weight ratio of the copper powder:aluminum powder:silver powder:palladium powder:binder is (30-45):(30-45):(0.1-5):(0.01-0.2):(10-40).
2. The method according to claim 1, wherein: The concentration of the nitric acid is 1-10wt%.
3. The method according to claim 1 or 2, wherein: In step (1), the weight ratio of the binder to nitric acid is 1:(0.5-1.5).
4. The method according to claim 3, wherein: In step (1), the weight ratio of the copper powder: aluminum powder: silver powder: palladium powder: binder is (35-42): (35-45): (0.2-2): (0.01-0.1): (16-30); And / or, the weight ratio of the binder: nitric acid is 1: (1-1.2).
5. The method according to claim 1 or 2, wherein: In step (2), the calcination conditions include: temperature of 600-1000° C.; time of 1-10 h.
6. The method according to claim 5, wherein: In step (2), the calcination conditions include: temperature of 600-800°C; time of 5-8h.
7. The method according to claim 1 or 2, wherein: In step (3), the caustic soda is sodium hydroxide and / or potassium hydroxide; And / or, the concentration of the caustic alkali aqueous solution is 2-40wt%.
8. The method according to claim 7, wherein: In step (3), the caustic soda is sodium oxide; And / or, the concentration of the caustic alkali aqueous solution is 10-30wt%.
9. The method according to claim 8, wherein: In step (3), the weight ratio of the calcined product to the caustic soda is 1:(1-3).
10. The method according to claim 9, wherein: In step (3), the weight ratio of the calcined product to the caustic soda is 1:(1-2).
11. The method according to claim 7, wherein: In step (3), the conditions for extracting aluminum include: temperature of 20-100°C; time of 0.5-2h.
12. The method according to claim 11, wherein: In step (3), the conditions for extracting aluminum include: temperature of 50-90°C; time of 1-2h.
13. The method according to any one of claims 8 to 10, wherein: In step (3), the conditions for extracting aluminum include: temperature of 20-100°C; time of 0.5-2h.
14. The method according to claim 13, wherein: In step (3), the conditions for extracting aluminum include: temperature of 50-90°C; time of 1-2h.
15. The method according to any one of claims 1-2, 4, 6, 8-12, 14, wherein: The method further comprises, before the molding process, performing the following steps: Copper powder, aluminum powder, silver powder and palladium powder are mixed, and then a binder and nitric acid are added and kneaded to obtain a plastic body.
16. The method according to claim 3, wherein: The method further comprises, before the molding process, performing the following steps: Copper powder, aluminum powder, silver powder and palladium powder are mixed, and then a binder and nitric acid are added and kneaded to obtain a plastic body.
17. The method according to claim 5, wherein: The method further comprises, before the molding process, performing the following steps: Copper powder, aluminum powder, silver powder and palladium powder are mixed, and then a binder and nitric acid are added and kneaded to obtain a plastic body.
18. The method according to claim 7, wherein: The method further comprises, before the molding process, performing the following steps: Copper powder, aluminum powder, silver powder and palladium powder are mixed, and then a binder and nitric acid are added and kneaded to obtain a plastic body.
19. The method according to claim 13, wherein: The method further comprises, before the molding process, performing the following steps: Copper powder, aluminum powder, silver powder and palladium powder are mixed, and then a binder and nitric acid are added and kneaded to obtain a plastic body.
20. A palladium-silver doped Raney copper catalyst prepared by the method according to any one of claims 1 to 19.
21. A method for preparing 1-butene by selective hydrogenation of C4 raffinate, characterized in that: include: The C4 raffinate is contacted with a catalyst for hydrogenation reaction to obtain 1-butene; wherein the C4 raffinate contains 1,3-butadiene; the catalyst is the palladium-silver doped Raney copper catalyst as claimed in claim 20; The conditions of the hydrogenation reaction include: the molar ratio of hydrogen to 1,3-butadiene is (0.2-10):1, the reactor inlet temperature is 30-60°C, the reaction pressure is 0.5-3MPa, and the reaction space velocity measured by the liquid volume of C4 raffinate is 2-20h -1 .
Citation Information
Patent Citations
Fixed-bed raney metal catalyst, its preparation and the hydrogenation of polymers using this catalyst
CA2216802A1
C4 hydrocarbon catalytic distillation method
CN104513119A
Silver modified raney copper catalyst, preparation method thereof and method for selective acetylene hydrogenation of C-4 fraction
CN106552647A
Method for catalyzing selective hydrogenation of 1,3-butadiene with PdAgCu / N-C catalyst
CN108786880A
Novel Raney copper catalyst as well as preparation method and application thereof
CN112264044A