A catalyst and its preparation method and application

By loading Co2P nanocomposites on modified Eloshi nanotubes modified with carbon dots, the problems of insufficient catalyst activity and high cost are solved, and efficient catalytic ammonia borane hydrolysis reaction under normal temperature and pressure are achieved, and hydrogen is improved storage and release efficiency.

CN116037172BActive Publication Date: 2024-11-15ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310084243.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-15
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

The existing catalysts have problems of insufficient activity and high cost in catalytic ammonia borane hydrolysis reaction, especially when there is no catalyst at room temperature and pressure, which affects the safe and efficient storage and release of hydrogen.

Method used

The Co2P nanocomposite material supported on modified Elostone nanotubes modified as catalyst was used to synthesize carbon dots and modified Elostone nanotubes by hydrothermal method, and the Co2P nanoparticles were fixed through EDC/NHS reaction. Improve the activity and stability of the catalyst.

Benefits of technology

Under normal temperature and pressure, the TOF value reaches 89.01 molH2molcat-1min-1 and the activation energy is 44.89kJ mol-1, which significantly improves the catalytic performance and stability of the catalyst and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116037172B_ABST
    Figure CN116037172B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of catalyst technology, and discloses a catalyst and a preparation method and application thereof, wherein the catalyst is a Co2P nanocomposite material supported on modified HNTs modified by CDs, and is recorded as Co2P-mHNTs / CDs. The method includes synthesizing CDs, modifying HNTs, synthesizing mHNTs / CDs, and synthesizing Co2P-mHNTs / CDs. The catalyst prepared by the present invention is used for catalyzing AB hydrolysis reaction, and has excellent catalytic performance. In an aqueous solution at room temperature and pressure, the TOF value reaches a maximum value of 89.01 mol H2 mol cat ‑ 1 min ‑1 , the activation energy is 44.89 kJ mol ‑1 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts and discloses a catalyst and a preparation method and application thereof. Background Art

[0002] As fossil energy is depleted, people are increasingly interested in hydrogen energy. Hydrogen is a green and sustainable energy source, but safe and efficient hydrogen storage technology remains a major problem that needs to be solved for its practical application. Traditional hydrogen storage methods include physical hydrogen storage and chemical hydrogen storage. Compared with physical hydrogen storage, chemical hydrogen storage is safer and more efficient, and is easier to achieve large-scale industrial applications. Ammonia borane (AB) has a high hydrogen storage capacity (19.6wt%), is non-toxic, easily soluble in water, and has a low molecular weight. It is a very promising chemical hydrogen storage material. In the presence of a suitable catalyst, 1 mol of AB can be completely hydrolyzed to release 3 mol of hydrogen. In this process, the hydrolysis reaction is thermodynamically feasible, but at room temperature and pressure, the hydrolysis reaction will not occur without the addition of a catalyst.

[0003] In recent years, both precious metals and non-precious metals have been widely and deeply studied in catalyzing AB hydrolysis. There is no doubt that precious metals perform significantly better than non-precious metals in catalytic dehydrogenation. However, in industrial catalysis, cost is a crucial consideration, so precious metal catalysts are not the most cost-effective choice. In recent years, transition metals have increasingly appeared in the field of catalysis, such as metal-based phosphides, oxides, nitrides, etc. In particular, transition metal phosphides have been widely studied due to their proper electron transfer from metal to P and good stability. For example, NiCoP supported on oxygen-doped porous carbon (OPC-300) has good catalytic performance for AB hydrolysis, with a TOF value of 95.24 mol / L in an alkaline environment. H2 mol cat -1 min -1 The electronic interactions between Ni, Co, P and the support OPC-300 enhanced the catalytic activity for AB hydrolysis. However, the agglomeration tendency of the nanoparticles during the phosphating process was not conducive to the improvement of the catalytic activity because the phosphating process may lead to a reduction in the surface area for the reaction.

[0004] Therefore, it is crucial to develop a stable and highly active catalyst. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a catalyst and a preparation method and application thereof.

[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0007] A catalyst is a Co2P nanocomposite material supported on modified HNTs (halloysite nanotubes) modified by CDs (carbon dots), which is denoted as Co2P-mHNTs / CDs.

[0008] The present invention also includes a method for preparing a catalyst, comprising the following steps:

[0009] S1, Synthetic CDs

[0010] Using poplar fluff as raw material, CDs solution was synthesized by hydrothermal method;

[0011] S2, Modification of HNTs

[0012] HNTs were added to an APTES-toluene mixed solution and subjected to ultrasonic treatment to obtain a suspension A; the suspension A was refluxed and then cooled to room temperature, and then centrifuged to obtain a solid A; the solid A was washed and dried to obtain amino-modified HNTs, which were recorded as mHNTs;

[0013] S3, Synthesis of mHNTs / CDs

[0014] CDs immobilized on mHNTs were prepared by connecting carboxyl and amino groups using EDC / NHS reaction, denoted as mHNTs / CDs;

[0015] S4, Synthesis of Co2P-mHNTs / CDs

[0016] NaPO2H2·H2O was dissolved in deionized water, and mHNTs / CDs were added. After ultrasonic treatment, a uniform suspension B was obtained. Then, under continuous stirring, Co(NO3)2·6H2O aqueous solution was added to the suspension B and stirring was continued. Finally, an excess amount of NaBH4 aqueous solution was added, stirred until no bubbles were generated, and solid C was obtained by centrifugation. Solid C was washed and dried to obtain Co2P-mHNTs / CDs.

[0017] Preferably, the process of step S1 is as follows: fully dispersing the cleaned poplar fluff into deionized water, cooling to room temperature after hydrothermal reaction, and filtering to obtain a filtrate; filtering the filtrate using a filter membrane, and then dialyzing using a dialysis bag to obtain a CDs solution.

[0018] Preferably, in step S1, the temperature of the hydrothermal reaction is 453K, the reaction time is 8h; the filter membrane is a 0.22μm filter membrane; the dialysis bag is a 500Da dialysis bag, and the dialysis time is 24h;

[0019] The mass volume ratio of the poplar fluff to deionized water is 1 g:60 mL.

[0020] Specifically, step S1 is to add 1 g of poplar fluff washed with ethanol to 60 mL of deionized water, and stir thoroughly until the mixture is evenly dispersed. Then, the mixture is hydrothermally reacted at 453 K for 8 h. After the reaction system is cooled to room temperature, the yellow filtrate is filtered to obtain a yellow filtrate, and the yellow filtrate is filtered through a 0.22 μm filter membrane, and then dialyzed with a 500 Da dialysis bag for 24 h to obtain a light yellow CDs solution.

[0021] Preferably, in step S2, the mass volume ratio of HNTs, APTES and toluene is 0.6 g:2 mL:25 mL; the ultrasonic treatment time is 30 min; the reflux temperature is 393 K, and the reflux time is 24 h; and the drying temperature is 343 K.

[0022] Specifically, step S2 is to add 2 mL of APTES (3-aminopropyltriethoxysilane) to 25 mL of toluene to obtain an APTES-toluene mixed solution, then add 0.6 g of HNTs to the APTES-toluene mixed solution, and ultrasonicate for 30 minutes to obtain a suspension. The suspension is then refluxed at 393K for 24 hours. After cooling to room temperature, solid A is obtained by centrifugation, and the obtained solid A is washed several times with toluene, and finally dried at 343K to obtain amino-modified HNTs, which are recorded as mHNTs.

[0023] Preferably, the process of step S3 is as follows: under vigorous stirring, EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride) and NHS (N-hydroxysuccinimide) are added to the CDs solution, and then mHNTs are added to the above solution, and vigorous stirring is continued to obtain a mixed solution; the mixed solution is centrifuged to obtain solid B, and the solid B is washed and dried to obtain mHNTs / CDs.

[0024] Preferably, in step S3, the volume mass ratio of CDs solution, EDC and NHS is 30 mL:15 mg:18 mg.

[0025] Specifically, step S3 is to add 15 mg EDC and 18 mg NHS to 30 mL CDs solution under vigorous stirring. Then, 100 mg mHNTs are added to the above solution, and the solution is stirred vigorously for 4 hours to obtain a mixed solution; the mixed solution is centrifuged to obtain solid B, and the solid B is fully washed with deionized water and dried in vacuum at 333K overnight to obtain mHNTs / CDs.

[0026] Preferably, in step S4, the ratio of NaPO2H2·H2O, mHNTs / CDs, and Co(NO3)2·6H2O is 2g:100mg:0.1-0.5mmol.

[0027] Specifically, step S4 is to dissolve 2g NaPO2H2·H2O in 20mL deionized water, then add 100mg mHNTs / CDs, and ultrasonicate for 30min to obtain a uniform suspension. Then, under continuous stirring, add dropwise 0.1-0.5mmol of 1mol L -1 The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1 The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain the black powder, which was Co2P-mHNTs / CDs.

[0028] The present invention also includes the use of the catalyst in the hydrolysis reaction of ammonia borane.

[0029] The working principle of the present invention:

[0030] HNTs (Halloysite Nanotubes) are a natural silicate clay mineral nanomaterial with a molecular formula of Al2Si2O5(OH)4·nH2O. HNTs are a natural clay-silicate mineral material with abundant reserves, environmental friendliness and low cost, and are used as catalyst carriers in the present invention. CDs (Carbon Dots) are a new type of carbon nanomaterial with the advantages of low preparation cost, simple synthesis method, high conductivity and easy surface modification.

[0031] The inventors studied the use of HNTs as carriers to load metal or metal phosphide catalysts for AB hydrolysis to produce hydrogen, and achieved good results. However, they are still looking for better methods to improve the catalytic activity of catalysts prepared using HNTs as catalyst carriers. It was found that HNTs as catalyst carriers have a good dispersion effect on transition metal phosphides, which can greatly improve their catalytic performance. In addition, the interaction between the carbon carrier and the phosphide makes the phosphide have strong catalytic performance in AB hydrolysis. The inventors studied the use of Ni 0.13 Co 0.87P was loaded on HNTs and Cu3P / Co2P was fixed in the C layer, and then the performance of AB hydrolysis and hydrogen production was tested. The results showed the excellence of supported transition metal phosphides for AB hydrolysis. In order to further improve the performance of catalytic AB hydrolysis, the inventors imagined whether CDs could be used to modify HNTs to improve the activity of the catalyst. There are many raw materials for synthesizing CDs, but there are not many reports on the preparation of CDs using waste biomass as raw materials. Using waste biomass as raw materials has the advantages of a wide source of raw materials and recycling of waste resources. Therefore, the inventors tried to modify HNTs with CDs prepared from poplar fluff, and then loaded the metal active components onto the CDs-modified HNTs, hoping to obtain excellent AB hydrolysis performance.

[0032] In the present invention, the inventors designed and synthesized a Co2P nanocomposite material loaded on modified HNTs modified with CDs. The present invention uses biomass material poplar fluff as a carbon source, obtains CDs by hydrothermal reaction, and then uses a typical EDC / NHS reaction to compound CDs with HNTs modified with a silane coupling agent to obtain mHNTs / CDs, and finally loads Co2P on mHNTs / CDs by liquid phase reduction. The prepared catalyst is used to catalyze the AB hydrolysis reaction and has excellent catalytic performance. In an aqueous solution at room temperature and pressure, the TOF value reaches a maximum value of 89.01 mol H2 mol cat -1 min -1 , the activation energy is 44.89 kJ mol -1 .

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention obtains a Co2P nanocomposite material Co2P-mHNTs / CDs loaded on a modified HNTs modified with CDs. The present invention uses biomass material poplar fluff as a carbon source, obtains CDs by hydrothermal reaction, and then uses a typical EDC / NHS reaction to compound CDs with HNTs modified with a silane coupling agent to obtain mHNTs / CDs, and finally loads Co2P on mHNTs / CDs by a liquid phase reduction method. The prepared catalyst is used to catalyze the AB hydrolysis reaction and has excellent catalytic performance. In an aqueous solution at room temperature and pressure, the TOF value reaches a maximum value of 89.01 mol H2 mol cat -1 min -1 , the activation energy is 44.89 kJ mol -1 . BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1Schematic diagram of the synthesis of Co2P-mHNTs / CDs of the present invention;

[0036] Figure 2 1 is a characterization diagram of CDs obtained in step S1 in Example 1 of the present invention; wherein Figure a is a TEM image of CDs, Figure b is an XRD spectrum of CDs, Figure c is an FT-IR spectrum of CDs, and Figure d is an ultraviolet absorption spectrum of CDs;

[0037] Figure 3 1 is a characterization diagram of Co2P-mHNTs / CDs obtained in step S4 in Example 1 of the present invention; wherein figure a is a TEM image of Co2P-mHNTs / CDs, figures bc are HRTEM images of Co2P-mHNTs / CDs, and figures dg are EDX element mapping images of Co2P-mHNTs / CDs;

[0038] Figure 4 XRD spectra of mHNTs obtained in step S2, mHNTs / CDs obtained in step S3, and Co2P-mHNTs / CDs obtained in step S4 in Example 1 of the present invention;

[0039] Figure 5 This is an X-ray photoelectron spectroscopy (XPS) analysis of Co2P-mHNTs / CDs obtained in step S4 in Example 1 of the present invention; wherein Figure a is an XPS spectrum of Co2P-mHNTs / CDs, Figure b is a high-resolution spectrum of C1s in Co2P-mHNTs / CDs, Figure c is a high-resolution spectrum of Co 2p in Co2P-mHNTs / CDs, and Figure d is a high-resolution spectrum of P 2p in Co2P-mHNTs / CDs;

[0040] Figure 6 The diagrams are the process diagrams and TOF value bar graphs of the catalysts with different initial metal Co addition amounts when catalyzing the hydrolysis of AB; wherein Figure a is the process diagram of the catalysts with different initial metal Co addition amounts when catalyzing the hydrolysis of AB, and Figure b is the TOF diagram corresponding to Figure a;

[0041] Figure 7 The performance curves and TOF value bar graphs of different catalysts for AB hydrolysis and hydrogen production; Figure a is the performance curves of different catalysts for AB hydrolysis and hydrogen production, and Figure b is the TOF value bar graph corresponding to Figure a;

[0042] Figure 8The performance graph of the amount of the catalyst Co2P-mHNTs / CDs obtained in Example 1 on the hydrolysis of AB; wherein Figure a is the performance curve of the Co2P-mHNTs / CDs catalyst for the hydrolysis of AB to produce hydrogen at 298K and different catalyst amounts, and Figure b is the relationship between the generation rate of H2 and the amount of the catalyst Co2P-mHNTs / CDs;

[0043] Fig. 9 The performance diagram of the catalyst Co2P-mHNTs / CDs obtained in Example 1 for the hydrolysis of AB at different temperatures; Figure a is the performance curve of Co2P-mHNTs / CDs catalyzing the hydrolysis of AB to produce hydrogen at different temperatures, and Figure b is the Arrhenius diagram obtained from the kinetic data;

[0044] Fig.10 The cycle performance test graph and TOF value bar graph of the catalyst Co2P-mHNTs / CDs obtained in Example 1; wherein Figure a is a cycle performance test graph of the catalyst Co2P-mHNTs / CDs, and Figure b is a TOF value bar graph corresponding to Figure a;

[0045] Fig.11 This is the mechanism diagram of hydrogen production by AB hydrolysis. DETAILED DESCRIPTION

[0046] The present invention is further described below with reference to specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0047] Example 1

[0048] A catalyst is a Co2P nanocomposite material supported on modified HNTs modified by CDs, which is denoted as Co2P-mHNTs / CDs.

[0049] like Figure 1 As shown, a method for preparing a catalyst comprises the following steps:

[0050] S1, Synthetic CDs

[0051] 1 g of poplar fluff washed with ethanol was added to 60 mL of deionized water and stirred thoroughly until uniformly dispersed. Then, the mixture was hydrothermally reacted at 453 K for 8 h. After the reaction system was cooled to room temperature, the yellow filtrate was filtered to obtain a yellow filtrate, which was then filtered through a 0.22 μm filter membrane and then dialyzed with a 500 Da dialysis bag for 24 h to obtain a light yellow CDs solution.

[0052] S2, Modification of HNTs

[0053] 2 mL of APTES was added to 25 mL of toluene to obtain an APTES-toluene mixed solution, and then 0.6 g of HNTs was added to the APTES-toluene mixed solution, and ultrasonicated for 30 min to obtain a suspension. The suspension was then refluxed at 393 K for 24 h. After cooling to room temperature, solid A was obtained by centrifugation, and the obtained solid A was washed with toluene several times, and finally dried at 343 K to obtain amino-modified HNTs, which were recorded as mHNTs.

[0054] S3, Synthesis of mHNTs / CDs

[0055] Under vigorous stirring, 15 mg EDC and 18 mg NHS were added to 30 mL CDs solution. Then 100 mg mHNTs were added to the above solution and continued to stir vigorously for 4 h to obtain a mixed solution. The mixed solution was centrifuged to obtain solid B, which was fully washed with deionized water and dried in vacuum at 333 K overnight to obtain mHNTs / CDs.

[0056] S4, Synthesis of Co2P-mHNTs / CDs

[0057] 2 g NaPO2H2·H2O was dissolved in 20 mL deionized water, and then 100 mg mHNTs / CDs was added. Ultrasonication was performed for 30 min to obtain a uniform suspension. Then, 0.3 mmol of 1 mol L -1 The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1 The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain the black powder, which was Co2P-mHNTs / CDs.

[0058] The Co2P-mHNTs / CDs obtained in this example is recorded as sample 3.

[0059] Example 2

[0060] Except for step S4, the remaining steps of this embodiment are the same as those of embodiment 1. Step S4 is specifically as follows:

[0061] S4, Synthesis of Co2P-mHNTs / CDs

[0062] 2 g NaPO2H2·H2O was dissolved in 20 mL deionized water, and then 100 mg mHNTs / CDs was added. Ultrasonication was performed for 30 min to obtain a uniform suspension. Then, 0.1 mmol of 1 mol L -1The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1 The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain the black powder, which was Co2P-mHNTs / CDs.

[0063] The Co2P-mHNTs / CDs obtained in this example is recorded as sample 1.

[0064] Example 3

[0065] Except for step S4, the remaining steps of this embodiment are the same as those of embodiment 1. Step S4 is specifically as follows:

[0066] S4, Synthesis of Co2P-mHNTs / CDs

[0067] 2 g NaPO2H2·H2O was dissolved in 20 mL deionized water, and then 100 mg mHNTs / CDs was added. Ultrasonication was performed for 30 min to obtain a uniform suspension. Then, 0.2 mmol of 1 mol L -1 The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1 The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain the black powder, which was Co2P-mHNTs / CDs.

[0068] The Co2P-mHNTs / CDs obtained in this example is recorded as sample 2.

[0069] Example 4

[0070] Except for step S4, the remaining steps of this embodiment are the same as those of embodiment 1. Step S4 is specifically as follows:

[0071] S4, Synthesis of Co2P-mHNTs / CDs

[0072] 2 g NaPO2H2·H2O was dissolved in 20 mL deionized water, and then 100 mg mHNTs / CDs was added. Ultrasonication was performed for 30 min to obtain a uniform suspension. Then, 0.4 mmol of 1 mol L -1 The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain the black powder, which was Co2P-mHNTs / CDs.

[0073] The Co2P-mHNTs / CDs obtained in this example is recorded as sample 4.

[0074] Example 5

[0075] Except for step S4, the remaining steps of this embodiment are the same as those of embodiment 1. Step S4 is specifically as follows:

[0076] S4, Synthesis of Co2P-mHNTs / CDs

[0077] 2 g NaPO2H2·H2O was dissolved in 20 mL deionized water, and then 100 mg mHNTs / CDs was added. Ultrasonication was performed for 30 min to obtain a uniform suspension. Then, 0.5 mmol of 1 mol L -1 The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1 The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain the black powder, which was Co2P-mHNTs / CDs.

[0078] The Co2P-mHNTs / CDs obtained in this example is recorded as sample 5.

[0079] Comparative Example 1

[0080] Preparation of Co2P-CDs: Dissolve 2g NaPO2H2·H2O in 20mL deionized water, then add 100mg CDs, and ultrasonicate for 30min to obtain a uniform suspension. Then, add 0.3mmol 1mol L -1 The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1 The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain a black powder, which was Co2P-CDs.

[0081] Comparative Example 2

[0082] Preparation method of Co2P-HNTs: 2g NaPO2H2·H2O was dissolved in 20mL deionized water, then 100mg HNTs was added, and ultrasonication was performed for 30min to obtain a uniform suspension. Then, 0.3mmol1mol L -1 The Co(NO3)2·6H2O aqueous solution was stirred for 12 h. Finally, an excess of 10 mol L -1 The mixture was stirred for 30 min until no bubbles were generated, centrifuged and washed with deionized water for several times, and dried in vacuum at 333 K overnight to obtain the black powder, which was Co2P-HNTs.

[0083] Comparative Example 3

[0084] Preparation method of Co2P-HNTs / CDs: 2g NaPO2H2·H2O was dissolved in 20mL deionized water, and then 100mg HNTs / CDs was added. (The preparation process of HNTs / CDs was as follows: 100mg HNTs was added to 45mL CDs solution under vigorous stirring, and continued to stir vigorously for 4h. Finally, the solid collected by centrifugation was fully washed with deionized water and vacuum dried at 333K overnight to obtain HNTs / CDs.) Ultrasonication for 30min was performed to obtain a uniform suspension. Then, under continuous stirring, 0.3mmol Co(NO3)2·6H2O aqueous solution was added dropwise, and stirring was continued for 12h. Finally, an excess of NaBH4 aqueous solution was added, and stirring was continued for 30min until no bubbles were generated, centrifuged and washed with deionized water several times, and vacuum dried at 333K overnight. The black powder obtained was Co2P-HNTs / CDs.

[0085] 1 Characterization of Co2P-mHNTs / CDs

[0086] TEM, HRTEM, XRD, XPS and ICP-AES were used to investigate the morphology, particle size, composition and electronic structure of the Co2P-mHNTs / CDs catalyst.

[0087] 1.1 A series of characterizations of CDs

[0088] like Figure 2 As shown, it is a characterization diagram of CDs obtained in step S1 in Example 1 of the present invention; wherein Figure a is a TEM image of CDs, Figure b is an XRD spectrum of CDs, Figure c is an FT-IR spectrum of CDs, and Figure d is an ultraviolet absorption spectrum of CDs.

[0089] like Figure 2As shown in Figure a, the morphology of the CDs synthesized in step S1 is characterized by TEM. The uniform distribution of ultrafine CDs nanoparticles can be clearly observed from TEM, and the average particle size of CDs is about 6 nm. Figure 2 As shown in Figure b, from the XRD spectrum of CDs, we can see that there is a broad peak at 22.4°, which corresponds to the diffraction peak of graphite carbon. Figure 2 As shown in Figure c, the Fourier transform infrared (FTIR) spectrum shows that at 3084 cm -1 There is a stretching vibration at 1713 cm -1 and 1408cm -1 The peaks at are C=O stretching vibration and CH deformation vibration. Figure 2 As shown in Figure d, at 339 nm, the ultraviolet absorption of the conjugated C=O and C=N bonds of CDs exhibits a typical nn* transition.

[0090] 1.2 A series of characterizations were performed on Co2P-mHNTs / CDs.

[0091] like Figure 3 As shown, it is a characterization diagram of Co2P-mHNTs / CDs obtained in step S4 in Example 1 of the present invention; wherein Figure a is a TEM image of Co2P-mHNTs / CDs, Figure bc is a HRTEM image of Co2P-mHNTs / CDs, and Figure dg is an EDX element mapping diagram of Co2P-mHNTs / CDs.

[0092] like Figure 3 As shown in Figure a, the morphology and nanoparticle size of Co2P-mHNTs / CDs were characterized by TEM, and it can be seen that the nanoparticles on the HNTs are evenly dispersed and the HNTs still maintain a complete tubular structure. Figure 3 As shown in Figures bc, the lattice fringes of carbon (0.338 nm) and Co2P (0.221 nm) can be seen from the HRTEM image of Co2P-mHNTs / CDs, confirming the successful preparation of the catalyst Co2P-mHNTs / CDs. Figure 3 As shown in the DG figure in the middle, the energy dispersive X-ray spectroscopy element mapping (EDX element mapping) also clearly shows the presence of elements C, Co, and P.

[0093] Table 1 shows the element content data of Co2P-mHNTs / CDs prepared with different initial amounts of added Co from Example 1 to Example 5 measured by ICP-AES.

[0094] Table 1 Element content data measured by ICP-AES

[0095]

[0096]

[0097] 1.3 X-ray diffraction (XRD) of Co2P-mHNTs / CDs

[0098] like Figure 4 The figure shows the XRD spectra of mHNTs obtained in step S2, mHNTs / CDs obtained in step S3, and Co2P-mHNTs / CDs obtained in step S4 in Example 1 of the present invention. The standard card in the figure is the standard card of Co2P: JCDPS 32-0306.

[0099] The XRD spectra of mHNTs, mHNTs / CDs, and Co2P-mHNTs / CDs all have peaks at 20.07°, 35.02°, 62.68°, and 73.79°, which correspond to the (100), (002), (110), (300), and (220) planes of HNTs, respectively. The XRD spectra of HNTs modified with APTES have the same peaks as the original HNTs, indicating that the combination of APTES and HNTs does not change the crystallinity of HNTs. After CDs functionalization, a new peak appears at 24.72°, confirming the successful combination of CDs and APTES-modified HNTs. In addition, after loading Co2P, new peaks appeared in the sample at 40.7°, 42.0°, and 43.3°, which correspond to the (121), (201), and (220) planes of Co2P, respectively, further confirming the successful loading of Co2P on mHNTs / CDs.

[0100] 1.4 X-ray photoelectron spectroscopy (XPS) analysis of Co2P-mHNTs / CDs

[0101] like Figure 5 As shown, it is the X-ray photoelectron spectroscopy (XPS) analysis of Co2P-mHNTs / CDs obtained in step S4 in Example 1 of the present invention; wherein Figure a is the XPS spectrum of Co2P-mHNTs / CDs, Figure b is the high-resolution spectrum of C1s in Co2P-mHNTs / CDs, Figure c is the high-resolution spectrum of Co2p in Co2P-mHNTs / CDs, and Figure d is the high-resolution spectrum of P 2p in Co2P-mHNTs / CDs.

[0102] In order to obtain the surface electronic information of Co2P-mHNTs / CDs, XPS spectrum analysis was performed. The XPS total spectrum of Co2P-mHNTs / CDs confirmed the presence of Al, Si, O, C, Co, and P elements. The C 1s spectrum can be decomposed into three peaks, representing different valence states of carbon atoms, namely C=O (288.60eV), CO (286.23eV), and CC (284.5eV). For the Co 2p high-resolution spectrum of Co2P-mHNTs / CDs, the binding energies at 778.8eV and 793.8eV are attributed to the binding energy of Co in Co2P, and the binding energies at 781.9eV and 791.8eV are attributed to the oxidation state of Co caused by oxidation of the catalyst surface. The P 2p spectrum can be decomposed into two peaks, PO (134.5eV) and MP (128.5eV).

[0103] Performance analysis of AB hydrolysis to produce hydrogen catalyzed by 2Co2P-mHNTs / CDs

[0104] The experiment adopts the "water drainage and gas collection method" to determine the rate of hydrogen production by the catalyst-catalyzed hydrolysis of AB. The specific test method is as follows: take the catalyst into a flask, add 2mL of deionized water, ultrasonicate for 30 minutes, and then preheat in a constant temperature water bath at 298K for 10 minutes, while checking the air tightness of the device, and then quickly inject the AB solution into the above system, and start timing at the same time. The two mouths on the left side of the flask are sealed with stoppers, and the outlet on the right end is connected to a burette filled with water. The amount of hydrogen released by the reaction can be determined by the drop in the water level in the burette. Until the liquid level in the burette no longer changes, it indicates that hydrogen production has ended and the reaction has stopped.

[0105] 2.1 Effect of different ratios of metal Co addition and carrier on catalytic performance

[0106] like Figure 6 As shown, these are the process diagrams and TOF diagrams of AB hydrolysis catalyzed by the catalysts with different initial metal Co addition amounts; Figure a is the process diagram of AB hydrolysis catalyzed by the catalysts with different initial metal Co addition amounts, and Figure b is the TOF diagram corresponding to Figure a.

[0107] Under the condition of a constant temperature water bath at a temperature of 298K, the ratio of metal to carrier was adjusted by changing the initial addition amount of metal Co, and its influence on the catalytic performance was studied. That is, a series of studies were carried out using the catalysts obtained in Examples 1 to 5 with different initial addition amounts of metal Co.

[0108] As can be seen from the figure, during the synthesis process, under the condition that the amount of carrier remains unchanged, as the initial amount of metal increases, the rate of catalytic AB hydrolysis continues to increase. However, the TOF value of the catalyst shows a volcano curve trend ( Figure 6(b) When the initial metal addition amount is between 0.1mmol and 0.3mmol, the TOF value increases with the increase of metal addition amount. When the metal addition amount is 0.3mmol, the TOF value reaches a peak value of 89.01mol H2 mol cat -1 min -1 Subsequently, as the amount of metal added increased, the TOF value gradually decreased (n was maintained during the test). Co2P / n AB =0.024 unchanged). This may be because excessive addition of initial metal will lead to agglomeration of metal nanoparticles during the synthesis process, resulting in a reduction in exposed active sites. Therefore, in the following experiments, the catalyst (obtained in Example 1) was synthesized according to the ratio of 100 mg mHNTs / CDs to 0.3 mmol metal Co, and a series of subsequent performance tests were performed.

[0109] 2.2 Investigation of synergistic effects in Co2P-mHNTs / CDs

[0110] A comparative study was conducted on the Co2P-mHNTs / CDs obtained in Example 1, the Co2P-CDs obtained in Comparative Example 1, the Co2P-HNTs obtained in Comparative Example 2, and the Co2P-HNTs / CDs obtained in Comparative Example 3.

[0111] like Figure 7 As shown, the performance curves and TOF graphs of different catalysts for AB hydrolysis and hydrogen production; Figure a is the performance curve of different catalysts for AB hydrolysis and hydrogen production, and Figure b is the TOF graph corresponding to Figure a.

[0112] Under the condition of 298K constant temperature water bath, the effects of different catalysts on the AB hydrolysis reaction to produce hydrogen were studied, such as Figure 7 In order to verify the unique performance of Co2P-mHNTs / CDs (obtained in Example 1), a control experiment was conducted.

[0113] When there is only CDs-Co2P, the activity of the catalyst is relatively poor, and it takes about 3.5 minutes to completely release 3 equivalents of H2. The catalytic performance of Co2P-HNTs is relatively good, and it takes about 1.5 minutes to complete the reaction. Co2P-HNTs / CDs (Comparative Example 3) obtained by physically mixing HNTs and CDs and loading Co2P did not significantly improve the catalytic activity of the catalyst, which may be because CDs did not effectively combine with HNTs.

[0114] Example 1 Co2P-mHNTs / CDs were obtained. The APTES-modified HNTs were compounded with CDs by EDC / NHS reaction, and then Co2P was loaded. It showed excellent catalytic activity. It only took about 0.5 min to completely complete the hydrolysis reaction and release 3 equivalents of H2. The TOF value reached 89.01 mol H2 mol cat -1 min -1 .

[0115] This shows that the interaction between CDs and metals can improve the activity of the catalyst. This effect is that CDs can enhance the electronic interaction between metal active components, promote electron transfer in the catalytic process, and thus improve the catalytic activity of the catalyst. When the Co2P / CDs complex is dispersed on HNTs, the catalytic activity is significantly improved, which is due to the higher dispersion of the catalyst active components and the exposure of more active sites when HNTs are used as carriers.

[0116] 2.3 Effect of Co2P-mHNTs / CDs dosage and reaction temperature on catalytic performance

[0117] The catalyst Co2P-mHNTs / CDs obtained in Example 1 was used for the experiment.

[0118] like Figure 8 As shown, it is a performance diagram of the effect of the amount of catalyst Co2P-mHNTs / CDs obtained in Example 1 on the hydrolysis of AB; wherein Figure a is a performance curve of the Co2P-mHNTs / CDs catalyst for hydrogen production by hydrolysis of AB at 298K and different catalyst amounts, and Figure b is the relationship between the H2 generation rate and the amount of catalyst Co2P-mHNTs / CDs.

[0119] This experiment studied the hydrolysis kinetics of AB. The hydrolysis kinetics of AB was further revealed by changing the amount of catalyst. Figure 8 It can be seen that when the amount of catalyst Co2P-mHNTs / CDs is between 5mg and 25mg, the reaction rate becomes faster and faster as the amount of catalyst increases. In order to balance the cost and performance of the catalyst, a catalyst amount of 10mg was used in the following experiments. Plotting ln[cat] against lnk, the slope after linear fitting is 1.07. The fitting results show that as the amount of catalyst increases, the reaction conforms to first-order kinetics.

[0120] like Fig. 9As shown, the performance graph of the catalyst Co2P-mHNTs / CDs obtained in Example 1 for the hydrolysis of AB at different temperatures; wherein Figure a is the performance curve of Co2P-mHNTs / CDs catalyzing the hydrolysis of AB to produce hydrogen at different temperatures, and Figure b is the Arrhenius graph obtained from the kinetic data. The catalyst Co2P-mHNTs / CDs was prepared in Example 1, and the amount of the catalyst used was 10 mg.

[0121] In order to study the effect of temperature on the hydrolysis rate of AB, the apparent activation energy (E a ), and the hydrolysis reaction rate at 298K-318K was also investigated ( Fig. 9 ). As the reaction temperature increases, the reaction rate increases. According to the linear fitting of 1 / T and Arrhenius equation, the E of the reaction is obtained. a The value is 44.89 kJ mol -1 , which is lower than the E of most non-precious metal catalysts a value.

[0122] 2.4 Stability study of Co2P-mHNTs / CDs

[0123] like Fig.10 As shown, it is a cycle performance test graph and a TOF value bar graph of the catalyst Co2P-mHNTs / CDs obtained in Example 1; wherein Figure a is a cycle performance test graph of the catalyst Co2P-mHNTs / CDs (in the figure, 1st is cycle 1, 2nd is cycle 2, 3rd is cycle 3, 4th is cycle 4, and 5th is cycle 5), and Figure b is a TOF value bar graph corresponding to Figure a.

[0124] In actual production applications, the stability and reusability of the catalyst are important indicators to measure the quality of the catalyst, so the stability and reusability of Co2P-mHNTs / CDs were also studied. Through experiments, it was found that the activity of the Co2P-mHNTs / CDs catalyst decreased with the increase in the number of cycles. After 5 cycles, the activity of the catalyst dropped to 50% of the initial level. During the reaction process, the decrease in catalyst activity is inevitable, and its decrease in activity may be due to the agglomeration of catalyst nanoparticles, the enlargement of catalyst particles, or the corrosion of the catalyst by the byproduct metaboric acid produced by the reaction.

[0125] Study on the reaction mechanism of AB hydrolysis to produce hydrogen over 3Co2P-mHNTs / CDs catalyst

[0126] like Fig.11 As shown, the mechanism diagram of AB hydrolysis to produce hydrogen.

[0127] In the present invention, the mechanism of AB hydrolysis catalyzed by Co2P-mHNTs / CDs catalyst is as follows: With mHNTs-CDs as carriers, an effective interface interaction can be formed between the catalyst and CDs, which can not only anchor Co2P but also promote charge transfer, and Co2P can expose a large surface area as an active site. In addition, the synergistic electronic effect between Co2P and the carrier plays a role, resulting in its strong adsorption of AB, effectively stimulating the BN bond in AB, thereby reducing the reaction energy barrier. The BN bond in AB dissociates to form B-OH under the oxidation of hydroxyl. The formation of the BN bond is inevitable, and the breaking and formation of the BN bond is another decisive step in the oxidative addition process of water. The formation of the B-OH bond must go through the dissociation process of the BN bond. Then, after the BH bond decomposes and produces a hydrogen, the BN bond needs to be reformed for the next round of hydroxyl addition.

[0128] In summary, the present invention successfully synthesized Co2P nanocomposites loaded on CDs-modified HNTs for the first time, and studied the morphology, structure, AB hydrolysis hydrogen production performance and AB hydrolysis kinetics of the synthesized catalyst. The main conclusions are as follows:

[0129] (1) The morphology of the synthesized Co2P-mHNTs / CDs catalyst was characterized. Co2P nanoparticles were evenly distributed on the surface of mHNTs / CDs, and the presence of C, Co, and P in the catalyst was confirmed. In addition, lattice fringes of C and Co2P were observed, further confirming the composition of the catalyst.

[0130] (2) The performance of Co2P-mHNTs / CDs in catalyzing AB hydrolysis was tested. Through a series of control experiments, it was found that when the metal loading was 10.15wt%, the catalyst had the best performance, with a TOF value of 89.01mol H2 mol cat -1 min -1 , which is higher than most transition metal catalysts. In addition, the interaction between metal and carbon can improve the catalytic activity. Using HNTs and CDs as carriers makes the active components in the catalyst more dispersed, thereby greatly improving the catalytic activity.

[0131] (3) Finally, the kinetics of the catalyst on the AB hydrolysis reaction was investigated. By changing the amount of catalyst used in the experiment, it was calculated that the reaction conformed to the first-order reaction kinetics. By testing the performance of the catalyst on the AB hydrolysis reaction at different temperatures, the Arrhenius equation showed that the Ea value of the reaction was 44.89 kJ mol -1 .

[0132] This provides a new idea for the synthesis of efficient and low-cost metal nanocatalysts for catalyzing AB hydrolysis.

[0133] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A method for preparing a catalyst, Features: The catalyst is Co supported on modified halloysite nanotubes HNTs modified with carbon dots CDs. 2 P nanocomposite material, denoted as Co 2 P-mHNTs / CDs; The following steps are involved: S1, Synthetic CDs Using poplar fluff as raw material, CDs solution was synthesized by hydrothermal method; S2, Modification of HNTs HNTs were added to an APTES-toluene mixed solution and subjected to ultrasonic treatment to obtain a suspension A; the suspension A was refluxed and then cooled to room temperature, and then centrifuged to obtain a solid A; the solid A was washed and dried to obtain amino-modified HNTs, which were recorded as mHNTs; S3, Synthesis of mHNTs / CDs CDs immobilized on mHNTs were prepared by connecting carboxyl and amino groups using EDC / NHS reaction, denoted as mHNTs / CDs; S4, Co 2 Synthesis of P-mHNTs / CDs NaPO 2 H 2 ·H 2 O was dissolved in deionized water, and mHNTs / CDs were added. After ultrasonication, a uniform suspension B was obtained. Then, Co(NO 3 ) 2 6H 2 O aqueous solution and continue stirring; finally, add excess NaBH 4 The aqueous solution was stirred until no bubbles were generated, and solid C was obtained by centrifugation; solid C was washed and dried to obtain Co 2 P-mHNTs / CDs; The process of step S1 is as follows: fully dispersing the cleaned poplar fluff into deionized water, cooling to room temperature after hydrothermal reaction, and filtering to obtain a filtrate; filtering the filtrate with a filter membrane, and then dialyzing with a dialysis bag to obtain a CDs solution; the filter membrane is a 0.22 μm filter membrane; the dialysis bag is a 500 Da dialysis bag; the mass volume ratio of the poplar fluff to the deionized water is 1 g:60 mL; In step S2, the mass volume ratio of HNTs, APTES, and toluene is 0.6 g:2 mL:25 mL; The process of step S3 is as follows: under the condition of vigorous stirring, EDC and NHS are added to the CDs solution, and then mHNTs are added to the above solution, and the vigorous stirring is continued to obtain a mixed solution; the mixed solution is centrifuged to obtain a solid B, and the solid B is washed and dried to obtain mHNTs / CDs; the volume mass ratio of the CDs solution, EDC, and NHS is 30mL:15mg:18mg; In step S4, NaPO 2 H 2 ·H 2 O, mHNTs / CDs, Co(NO 3 ) 2 6H 2 The ratio of O is 2g:100mg:0.1-0.5mmol.

2. A method for preparing a catalyst according to claim 1, Features: In step S1, the temperature of the hydrothermal reaction is 453 K, the reaction time is 8 h, and the dialysis time is 24 h.

3. A method for preparing a catalyst according to claim 1, Features: In step S2, the ultrasonic treatment time is 30 minutes; the reflux temperature is 393K, the reflux time is 24 hours; and the drying temperature is 343K.

4. Use of the catalyst prepared by the preparation method according to any one of claims 1 to 3 in the hydrolysis reaction of ammonia borane.