Catalytic adsorbent for flue gas demercuration and denitrification, preparation method and application thereof, and method for treating flue gas from coal-fired power plant
By loading nano-Fe3O4 particles and CeO2 active component catalytic adsorbent on EVS-10 molecular sieve, the problem of synergistic removal of nitrogen oxides and mercury in the flue gas of coal-fired power plants is solved, achieving efficient flue gas treatment and low-cost Recycle.
Patent Information
- Application Number
- CN202111276247.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing technology cannot effectively remove nitrogen oxides and mercury from coal-fired power plant flue gas at the same time, and existing catalysts have problems such as low efficiency and easy agglomeration during repeated recycling processes.
The carrier is EVS-10 molecular sieve, and the catalytic adsorbent loaded with nano-Fe3O4 particles and CeO2 active components is recycled through a magnetic separation device to achieve coordinated removal of nitrogen oxides and mercury.
The catalytic adsorbent has efficient mercury removal and denitration performance, and is easy to recycle through a magnetic separation device, reducing the cost of use. It is suitable for use in series with dust removal and desulfurization equipment, and is suitable for flue gas treatment in coal-fired power plants.
Smart Images

Figure BDA0003330026500000121 
Figure BDA0003330026500000131
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of environmental protection and air pollution control, and in particular, to a catalytic adsorbent for flue gas demercuration and denitrification, a preparation method and application thereof, and a method for treating flue gas from a coal-fired power plant. Background Art
[0002] Nitrogen oxides and mercury are common substances in the flue gas of coal-fired power plants. Nitrogen oxides are a common air pollutant produced by coal combustion, which can cause acid rain and the greenhouse effect. x ) accounts for more than 95% of NO. The key to removing nitrogen oxides from flue gas is to remove NO to the greatest extent. Currently, the most effective and widely used technology for removing NO from coal-fired flue gas is NH3 selective catalytic reduction (SCR) technology. The SCR catalysts currently studied mainly use metal oxides such as V2O5, CuO, Cr2O3, CeO2, Fe2O3, MnO x , Co2O3, etc. are loaded on carriers such as Al2O3, SiO2, TiO2, ZrO2, carbon materials and molecular sieves. However, the molecular sieves used in the prior art cannot achieve effective mercury removal performance while removing nitrogen oxides; and are not conducive to repeated recycling.
[0003] Mercury is a toxic heavy metal. Mercury in flue gas is mainly in the form of Hg 2+ , Hg p and Hg 0 There are three forms, Hg 2+ It is soluble in water and can therefore be removed efficiently by the pollutant control equipment wet flue gas desulfurization device; Hg p Since it is combined with fly ash, it can be removed by particulate matter control equipment such as bag filters or electrostatic precipitators; however, Hg 0 It is insoluble in water and volatile, and is quite stable at low temperatures. It is difficult to be removed by the existing pollutant control equipment in power plants and is directly discharged into the atmosphere. Therefore, the key to removing mercury from flue gas in coal-fired power plants is to control Hg 0 The two main research directions of mercury removal are adsorbent demercuration and catalytic oxidation demercuration: Adsorbent demercuration is to remove Hg 0 Through physical or chemical adsorption to the adsorbent surface, and then removed by the particulate matter control equipment; catalytic oxidation demercuration is to remove Hg 0 Highly efficient oxidation to Hg 2+ , and then removed by the wet desulfurization device. Existing molecular sieves have a certain ability to catalytically oxidize elemental mercury, but the efficiency of catalytic oxidation of mercury is low (about 48%). In addition, molecular sieve catalysts do not have the performance of synergistic demercuration and denitrification; and they are easy to agglomerate into larger particles during repeated recycling.
[0004] In addition, the recycling of catalysts is also a problem. Magnetic particles are widely concerned because they are easy to separate from fluids and can be regenerated and recycled. Therefore, how to provide a catalytic adsorbent with magnetic properties and synergistic demercuration and denitrification is also worth further research. Summary of the invention
[0005] The purpose of the present disclosure is to provide a catalytic adsorbent for flue gas demercuration and denitrification, a preparation method and application thereof, and a method for treating flue gas from a coal-fired power plant. The catalytic adsorbent can remove mercury and nitrogen oxides and can be easily recycled by a magnetic separation device.
[0006] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a catalytic adsorbent for flue gas demercurization and denitrification, the catalytic adsorbent comprising a carrier, magnetic particles and an active component; the magnetic particles comprise nano-Fe3O4 particles and a silicon oxide layer coated on the surface of the nano-Fe3O4 particles, and the active component is loaded on the carrier; the carrier comprises EVS-10 molecular sieve, and the active component comprises CeO2.
[0007] Optionally, based on the total weight of the catalytic adsorbent, the mass fraction of the magnetic particles is 5 to 50% by weight, the mass fraction of the carrier is 35 to 94% by weight, and the mass fraction of the active component is 1 to 15%.
[0008] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps: (1) mixing a magnetic EVS-10 molecular sieve, a cerium source and water to obtain a raw material mixture, wherein the magnetic EVS-10 molecular sieve includes the carrier and the magnetic particles; (2) adding an alkaline solution to the raw material mixture for mixing, and then adding alcohol to obtain a colloidal precursor; (3) performing a first calcination treatment on the colloidal precursor; wherein the magnetic EVS-10 molecular sieve includes the EVS-10 molecular sieve and the magnetic particles.
[0009] Optionally, the mixing described in step (1) also includes adding a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, preferably polymethacrylic acid; optionally, the weight ratio of the dispersing aid to the cerium source is (30-70): (10-20); optionally, step (1) also includes: ultrasonically treating the magnetic EVS-10 molecular sieve in water for 5-30 minutes, and then adding the cerium source and the optional dispersing aid to mix to obtain a raw material mixture.
[0010] Optionally, the method also includes preparing the magnetic EVS-10 molecular sieve by the following steps: a. Mixing Fe3O4 particles, silicate solution and water, and then adding acid to adjust the pH, preferably adjusting to a pH of 9.3-9.7, to obtain a first mixture; b. Keeping the first mixture at 30-45°C for 2-4 hours; then heating to 85-95°C and keeping it for 1-2 hours; then cooling to room temperature; performing a first separation using a magnetic separation device to obtain a first solid product with magnetism; c. dispersing the EVS-10 molecular sieve and the first solid product in a solvent, performing a second separation to remove the solvent; and performing a second calcination treatment to obtain the magnetic EVS-10 molecular sieve.
[0011] Optionally, in step a, the weight ratio of the Fe3O4 particles, silicate and water is (0.45~0.9):1:(27~54); the silicate includes sodium silicate; further preferably, the concentration of the silicate solution is 0.5~3 mol / L; optionally, the acid is hydrochloric acid or sulfuric acid; further preferably, the concentration of the acid is 0.1~1 mol / L; optionally, step a includes: dispersing a suspension of the Fe3O4 particles and deionized water, the dispersing method including at least one of ultrasonic treatment and mechanical stirring, and then adding the silicate solution to the obtained dispersion system.
[0012] Optionally, in step c, the solvent is selected from one or more of toluene, acetone and ethyl acetate, preferably toluene; optionally, step c includes: adding the EVS-10 molecular sieve to the solvent for ultrasonic treatment, adding the first solid product and continuing ultrasonic treatment to obtain a suspension; then performing a second separation, optionally, the second separation includes: after the obtained suspension is allowed to stand for stratification, removing the upper layer of solvent, and then evaporating at 90-110°C to remove residual solvent; in step c, the conditions of the second calcination treatment include: a calcination temperature of 250-350°C and a calcination time of 1-2 hours.
[0013] Optionally, in step (1), the weight ratio of the magnetic EVS-10 molecular sieve, the cerium source and water is (90-5): (13-18): (50-60); the cerium source is a water-soluble cerium salt, preferably one or more selected from cerium acetate, cerium chloride and cerium nitrate.
[0014] Optionally, step (2) comprises: mixing the raw material mixture and the alkaline solution and ultrasonically treating them for 5 to 30 minutes, and then adding alcohol to obtain the colloidal precursor; wherein the alkaline solution comprises aqueous ammonia; and the alcohol comprises ethanol; and further preferably, the volume ratio of the alkaline solution and the alcohol added is (4 to 8): (60 to 70).
[0015] Optionally, in step (3), the conditions of the first calcination treatment include: under an inert atmosphere, a calcination temperature of 350 to 600°C and a calcination time of 1 to 4 hours; wherein the inert atmosphere is nitrogen or argon; the method also includes: before performing the first calcination treatment, ultrasonically treating the colloidal precursor for 5 to 30 minutes, and then evaporating it at 70 to 100°C.
[0016] The third aspect of the present disclosure provides application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0017] The fourth aspect of the present disclosure provides a method for treating flue gas from a coal-fired power plant, comprising contacting the flue gas containing mercury and NOx generated by the coal-fired power plant with the catalytic adsorbent described in the first aspect of the present disclosure, and then passing the contacted flue gas through a magnetic separation device to separate the flue gas from the catalytic adsorbent, and the flue gas enters a subsequent treatment process to recycle the catalytic adsorbent.
[0018] Through the above technical scheme, the present disclosure provides a catalytic adsorbent for flue gas demercurization and denitrification, and a preparation method and application thereof. The catalytic adsorbent is magnetic, can be effectively recycled, avoids secondary pollution of fly ash, and has low use cost. The present disclosure adopts EVS-10 molecular sieve as a carrier to load a highly dispersed CeO2 active component. The catalytic adsorbent has good mercury removal efficiency and denitrification efficiency, and can synergistically remove elemental mercury and nitrogen oxides in coal-fired flue gas. The catalytic adsorbent has improved resistance to sulfur poisoning, good process adaptability and compatibility, and is suitable for use in series with dust removal and desulfurization equipment. It is particularly suitable for enterprises with desulfurization and dust removal equipment to expand their use for demercurization upgrades, which reduces equipment installation and use costs and has prospects for industrial application.
[0019] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0020] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0021] A first aspect of the present disclosure provides a catalytic adsorbent for flue gas demercuration and denitrification, the catalytic adsorbent comprising a carrier, magnetic particles and an active component; the magnetic particles comprising nano Fe3O4 particles and a silicon oxide layer coated on the surface of the nano Fe3O4 particles, the active component being loaded on the carrier; the carrier comprising EVS-10 molecular sieve, and the active component comprising CeO2.
[0022] The catalytic adsorbent provided by the present invention is magnetic and can be recycled by a magnetic separation device (such as a high-gradient magnetic machine), thus avoiding secondary pollution of fly ash and having a low cost of use. The present invention adopts EVS-10 molecular sieve as a carrier to load CeO2 active components, and the CeO2 active components have a high degree of dispersion. The catalytic adsorbent has both excellent mercury removal efficiency and high denitrification efficiency, and can synergistically remove elemental mercury and nitrogen oxides in coal-fired flue gas. The catalytic adsorbent has good sulfur poisoning resistance, process adaptability and compatibility, and is suitable for use in series with dust removal and desulfurization equipment. It is particularly suitable for enterprises with desulfurization and dust removal equipment to expand their use for mercury removal upgrades, which reduces equipment installation and use costs and has prospects for industrial application.
[0023] In the present disclosure, the EVS-10 molecular sieve refers to a vanadium silicate molecular sieve, which is a type of molecular sieve in which vanadium completely replaces the titanium in the titanium silicate molecular sieve ETS-10. It has high hydrothermal stability, large specific surface area, fast heat and mass transfer, and is an excellent catalyst and carrier. The present disclosure uses the EVS-10 molecular sieve as a carrier. The molecular sieve skeleton contains a vanadium active component, which can catalytically oxidize part of the elemental mercury; the loaded CeO2 active component also has a good catalytic oxidation ability of elemental mercury and nitrogen oxides, and the two active components exert a synergistic catalytic oxidation effect. The inventor also found in the experiment that CeO2 as an active component is conducive to improving the resistance of catalytic adsorption to SO2 poisoning. The present invention discloses a catalytic adsorbent formed by combining an EVS-10 molecular sieve loaded with a CeO2 active component and nano-Fe3O4 particles coated with a silicon oxide layer on the surface, wherein the silicon oxide layer can not only protect the nano-Fe3O4 particles from maintaining their magnetism under complex conditions such as high temperature and acidity, but also play a connecting role, firmly bonding with the EVS-10 molecular sieve during the high-temperature sintering process, so that the catalytic adsorbent has good mercury removal and denitrification performance and is easy to recycle.
[0024] In one embodiment, based on the total weight of the catalytic adsorbent, the mass fraction of the magnetic particles is 5 to 50% by weight, the mass fraction of the carrier is 35 to 94% by weight, and the mass fraction of the active component is 1 to 15%. When the content of each component in the catalytic adsorbent provided by the present disclosure is within the range of this embodiment, the obtained catalytic adsorbent can achieve a better effect of synergistically removing elemental mercury and nitrogen oxides, and the recovery effect is better.
[0025] The specific form of the magnetic particles in the present disclosure is nano Fe3O4 particles coated with SiO2 on the surface, and specifically, the particle size of the magnetic particles is 50 to 200 nm. The content of the SiO2 layer in the present disclosure can vary within a wide range so that the mass fraction of the final magnetic particles in the entire catalytic adsorbent is 5 to 50 weight %.
[0026] In one embodiment, the carrier is an EVS-10 molecular sieve, and the molar ratio of Si:Na:K:V in the EVS-10 molecular sieve is 3.92:1.39:0.48:1, based on the molar amount of the elements. Specifically, the chemical composition of the EVS-10 molecular sieve can be determined by XRF spectroscopy.
[0027] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps:
[0028] (1) mixing a magnetic EVS-10 molecular sieve, a cerium source and water to obtain a raw material mixture, wherein the magnetic EVS-10 molecular sieve includes the carrier and the magnetic particles;
[0029] (2) adding an alkaline solution to the raw material mixture for mixing, and then adding alcohol to obtain a colloidal precursor;
[0030] (3) performing a first calcination treatment on the colloidal precursor;
[0031] The magnetic EVS-10 molecular sieve comprises the EVS-10 molecular sieve and the magnetic particles.
[0032] In a specific embodiment, the method provided in the present disclosure further comprises preparing the magnetic EVS-10 molecular sieve by the following steps:
[0033] a. Mixing Fe3O4 particles, a silicate solution and water, and then adding an acid to adjust the pH, preferably to a pH of 9.3 to 9.7, to obtain a first mixture;
[0034] b. Keeping the first mixture at 30-45° C. for 2-4 hours; then heating to 85-95° C. and keeping it for 1-2 hours; then cooling to room temperature; performing a first separation using a magnetic separation device to obtain a first solid product having magnetic properties;
[0035] c. Dispersing the EVS-10 molecular sieve and the first solid product in a solvent, performing a second separation to remove the solvent; and performing a second calcination treatment to obtain the magnetic EVS-10 molecular sieve.
[0036] Specifically, the magnetic separation device in the present disclosure can be an electromagnetic separation device, a magnet, or other device conventionally selected in the art.
[0037] The present invention firstly coats the Fe3O4 nanoparticles with a SiO2 layer through the above steps a and b, and firmly bonds with the EVS-10 molecular sieve during high-temperature sintering (the second calcination treatment) to obtain the magnetic EVS-10 molecular sieve.
[0038] Furthermore, the present invention first synthesizes the magnetic EVS-10 molecular sieve through the above steps and then loads CeO2, which can ensure that the loading of CeO2 is not affected, and further ensure that the final catalytic adsorbent has good magnetic properties and high mercury removal and denitrification performance.
[0039] The EVS-10 molecular sieve used in the present disclosure can be prepared by existing methods, for example, it can be prepared by the method disclosed in the document ZijianZhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0040] The EVS-10 molecular sieve used in the present disclosure can be prepared by a hydrothermal method. In a specific embodiment, the steps include: dissolving sodium silicate in deionized water; then adding NaOH, KCl, NaF and NaCl to the solution to obtain solution A. Then VOSO4 is dissolved in deionized water to obtain solution B. Solution A and solution B are mixed and stirred, and aged at room temperature. The aged mixture is transferred to an autoclave for further aging. The synthesized product is washed with deionized water and dried to obtain an EVS-10 molecular sieve. During the preparation process, the amount of each reactant and the reaction conditions can be adjusted according to actual needs.
[0041] In one embodiment, in step a, the weight ratio of the Fe3O4 particles, silicate and water is (0.45-0.9):1:(27-54);
[0042] The silicate includes sodium silicate; further preferably, the concentration of the silicate solution is 0.5 to 3 mol / L;
[0043] Optionally, the acid is hydrochloric acid or sulfuric acid; further preferably, the concentration of the acid is 0.1 to 1 mol / L;
[0044] Optionally, step a comprises: dispersing a suspension of the Fe3O4 particles and deionized water, wherein the dispersing method comprises ultrasonic treatment followed by mechanical stirring, and then adding the silicate solution to the obtained dispersion system.
[0045] In one embodiment, in step c, the solvent is selected from one or more of toluene, acetone and ethyl acetate, preferably toluene. The present invention uses an organic solvent such as toluene rather than an aqueous solution system to disperse the EVS-10 molecular sieve and the Fe3O4 nanoparticles coated with a thin layer of SiO2, which can prevent the SiO2 thin layer from dissolving and migrating to the surface of the molecular sieve, thereby causing blockage of the molecular sieve pores.
[0046] In an optional embodiment, step c includes: adding the EVS-10 molecular sieve to the solvent for ultrasonic treatment, adding the first solid product and continuing ultrasonic treatment to obtain a suspension; then performing a second separation, the second separation is, for example, allowing the obtained suspension to stand for stratification, removing the upper layer of solvent, and then evaporating at 90 to 110°C to remove the residual solvent.
[0047] In one embodiment, in step c, the conditions of the second calcination treatment include: a calcination temperature of 250 to 350° C. and a calcination time of 1 to 2 hours.
[0048] In one embodiment, in step (1), the weight ratio of the magnetic EVS-10 molecular sieve, the cerium source and water is (90-5): (13-18): (50-60); the cerium source is a water-soluble cerium salt, preferably one or more selected from cerium acetate, cerium chloride and cerium nitrate.
[0049] In a preferred embodiment, the mixing in step (1) further comprises adding a dispersing aid;
[0050] The dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, preferably polymethacrylic acid; the molecular weight of the dispersing aid in the present disclosure can vary within a wide range and can be selected according to actual needs.
[0051] In one embodiment, the weight ratio of the dispersing aid to the cerium source is (34-68): (13-18).
[0052] In one embodiment, step (1) further comprises: ultrasonically treating the magnetic EVS-10 molecular sieve in water for 5 to 30 minutes, and then adding the cerium source and the optional dispersing aid to mix to obtain a raw material mixture. The "ultrasonic treatment" described in this disclosure refers to ultrasonic treatment using a conventional ultrasonic instrument to make the material mixing or dispersion more uniform.
[0053] The present invention introduces a cerium source and a dispersing aid simultaneously during the process of preparing the catalytic adsorbent, which is beneficial to further improve the mercury removal and denitrification efficiency of the catalytic adsorbent.
[0054] The Ce ions form a complex with the dispersing agent, so that after the subsequent addition of an alkaline solution (such as ammonia water), the uniformly dispersed Ce complex can also stably exist in the system, avoiding agglomeration; after the addition of alcohol, the complex in the system forms a dispersing agent-Ce polymer particles (such as PMAA-Ce polymer particles) on the surface of the magnetic EVS-10 molecular sieve. The electrostatic repulsion between the particles makes the system very stable, ensuring the dispersion of the Ce ions, so that the particle size of the CeO2 loaded in the finally synthesized catalytic adsorbent is small and evenly distributed.
[0055] In one embodiment, step (2) comprises: mixing the raw material mixture and the alkaline solution and ultrasonically treating them for 5 to 30 minutes, and then adding alcohol to obtain the colloidal precursor; wherein the alkaline solution comprises aqueous ammonia; and the alcohol comprises ethanol; and further preferably, the volume ratio of the alkaline solution and the alcohol added is (4 to 8): (60 to 70).
[0056] In one embodiment, the method further comprises: before the first calcination treatment, subjecting the colloidal precursor to ultrasonic treatment for 5 to 30 minutes to enhance the precipitation effect of the cerium source in the colloidal precursor on the surface of the EVS molecular sieve; and then evaporating at 70 to 100° C. for drying.
[0057] In one embodiment, in step (2), the conditions of the first calcination treatment include: a calcination temperature of 350 to 600° C. and a calcination time of 1 to 4 hours under an inert atmosphere; wherein the inert atmosphere is nitrogen or argon.
[0058] The third aspect of the present disclosure provides application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0059] The fourth aspect of the present disclosure provides a method for treating flue gas from a coal-fired power plant, comprising contacting the flue gas containing mercury and NOx generated by the coal-fired power plant with the catalytic adsorbent described in the first aspect of the present disclosure, and then passing the flue gas after contact through a magnetic separation device to separate the flue gas from the catalytic adsorbent, and the flue gas enters a subsequent treatment process to recycle the catalytic adsorbent. The catalytic adsorption provided by the present disclosure can be effectively separated by using a magnetic device during the application process, which is conducive to recycling; and the catalytic adsorbent provided by the present disclosure can effectively catalyze the oxidation of elemental mercury through molecular sieves and active components, and the catalytic adsorbent does not adsorb elemental mercury, so the catalyst can be recycled without regeneration, which is more convenient.
[0060] The present invention is further described below in conjunction with specific embodiments, but the scope of protection claimed by the present invention is not limited to the scope described in the embodiments.
[0061] The chemicals used in each example can be obtained through public commercial channels.
[0062] The EVS-10 molecular sieve used in the following examples and comparative examples was prepared according to the method disclosed in Zijian Zhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0063] The 25% ammonia water used in the following examples and comparative examples is ammonia water having an NH3·H2O content of 25% by weight.
[0064] Ultrasonic treatment refers to the use of conventional ultrasonic instruments to mix and disperse uniformly.
[0065] Example 1
[0066] (1) A suspension of 2 g of Fe3O4 particles and 120 mL of deionized water was mechanically stirred at 40° C. 2.23 g of sodium silicate pentahydrate was dissolved in water to prepare 10 mL of a 1 mol / L sodium silicate solution, which was added to the suspension. Then 0.3 mol / L of sulfuric acid was added dropwise to control the pH of the solution to 9.5±0.2. The temperature was kept at 95° C. for 3 hours, and the temperature was kept at 95° C. for 1 hour. The temperature was then cooled to room temperature. The Fe3O4 particles coated with the SiO2 layer were separated by a magnet, washed twice with deionized water, and dried in a vacuum drying oven.
[0067] (2) 8 g of EVS-10 molecular sieve and toluene were ultrasonically treated and mixed, 2 g of Fe3O4 particles coated with SiO2 were added, and the ultrasonic treatment was continued. After the suspension was separated, the upper toluene liquid was poured out, and the remaining toluene was removed under vacuum. The lower solid was placed in a tubular furnace and calcined at 300°C for 1 hour under a nitrogen atmosphere, and sieved with a 100-mesh screen, and the particles under the sieve were taken to obtain a magnetic EVS-10 molecular sieve;
[0068] (3) 9.0 g of magnetic EVS-10 molecular sieve was dispersed in 50 mL of deionized water, and after ultrasonic treatment for 15 min, 1.8 g of (CH3CO2)3Ce hydrate and 6.8 g of polymethacrylic acid were added;
[0069] (4) Add 8 mL of 25% ammonia water and perform ultrasonic treatment for 15 minutes, then add 70 mL of ethanol to form a colloidal precursor. After continuing the ultrasonic treatment for 30 minutes, evaporate the sample at 80°C, and finally calcine the sample at 500°C in a muffle furnace for 2 hours. After cooling to room temperature, sieve to less than 100 mesh to obtain the final catalytic adsorbent, which is recorded as sample 1.
[0070] Comparative Example 1
[0071] The catalytic adsorbent was prepared by similar steps to Example 1, except that the EVS-10 molecular sieve was replaced with the ETS-10 molecular sieve. The other preparation steps were the same as those in Example 1, and a catalytic adsorbent was obtained, which was recorded as sample D-1.
[0072] Comparative Example 2
[0073] A preparation method similar to that of Example 1 was adopted, which differed from Example 1 in that only steps (1) and (2) in Example 1 were performed in this comparative example, and steps (3) and (4) were not performed, to obtain a magnetic EVS-10 molecular sieve, which was recorded as sample D-2.
[0074] Example 2
[0075] (1) A suspension of 1 g of Fe3O4 particles and 60 mL of deionized water was mechanically stirred at 40° C. 2.23 g of sodium silicate pentahydrate was dissolved in water to prepare 20 mL of a 0.5 mol / L sodium silicate solution, which was added to the suspension. Then 0.2 mol / L of hydrochloric acid was added dropwise to control the pH of the solution to 9.5±0.2. The temperature was kept at 95° C. for 3 hours, and the temperature was kept at 95° C. for 1 hour. The temperature was then cooled to room temperature. The Fe3O4 particles coated with a layer of SiO2 were separated by a magnet, washed twice with deionized water, and dried in a vacuum drying oven.
[0076] (2) 9g of EVS-10 molecular sieve and toluene were ultrasonically treated and mixed, 1g of Fe3O4 particles coated with SiO2 were added, and the ultrasonic treatment was continued. After the suspension was separated, the upper toluene liquid was poured out, and the remaining toluene was removed under vacuum. The lower solid was placed in a tube furnace and calcined at 300°C for 1 hour under a nitrogen atmosphere, and sieved with a 100-mesh screen, and the particles under the sieve were taken to obtain a magnetic EVS-10 molecular sieve;
[0077] (3) 9.5 g of magnetic EVS-10 molecular sieve was dispersed in 60 mL of deionized water, and after ultrasonic treatment for 15 min, 1.3 g of Ce(NO3)3·6H2O and 3.4 g of polymethacrylic acid were added;
[0078] (4) Add 4 mL of 25% ammonia water and ultrasonically treat for 15 minutes, then add 60 mL of ethanol to form a colloidal precursor. After continuing the ultrasonic treatment for 30 minutes, evaporate the sample at 80°C, and finally calcine the sample at 600°C in a muffle furnace for 2 hours. After cooling to room temperature, sieve to less than 100 mesh to obtain the final catalytic adsorbent, which is recorded as sample 2.
[0079] Example 3
[0080] A preparation method similar to that of Example 1 was used, except that no dispersing aid polymethacrylic acid was added in step (3), and the remaining preparation process and reaction parameters were the same as those of Example 1. The final catalytic adsorbent was obtained, which was recorded as Sample 3.
[0081] Comparative Example 3
[0082] Weigh 4.3 g of AgNO3 and dissolve it in 100 ml of deionized water, then add 10 g of EVS-10 molecular sieve, stir it magnetically in a dark environment for 6 h, then filter it, rinse it repeatedly with deionized water, dry it at 80 ° C, and then bake it in a tube furnace at 250 ° C in a nitrogen atmosphere for 1 hour. The catalytic adsorbent loaded with only silver nanoparticles is obtained, which is recorded as sample D-3.
[0083] The mass fractions of the carrier molecular sieve, active components, magnetic particles in the samples obtained from the above embodiments and comparative examples, as well as the mass fraction of silicon oxide in the magnetic particles are listed in the following Table 1.
[0084] Table 1
[0085]
[0086]
[0087] Simulated smoke test example
[0088] The samples synthesized in the above examples and comparative examples were placed in a simulated flue gas experimental system to test the demercuration and denitrification performance. The simulated flue gas conditions are as follows: 5% O2, 12% CO2, 400ppm NO, 400ppm NH3, 600ppm SO2, 30ppm HCl, Hg 0 Concentration: 110 μg / m 3 The balance gas is N2, the total flow rate of the test flue gas is 500 mL / min, and the test temperature is 250° C. The experimental system for simulating flue gas adopts the experimental system conventionally selected in the art. The results of the mercury removal and denitrification tests are listed in Table 2 below.
[0089] The samples synthesized in the examples and comparative examples were mixed with fly ash, and the separation performance was tested by magnet. The recovery rates of the catalytic adsorbent are listed in Table 2 below.
[0090] Table 2
[0091] sample <![CDATA[Hg 0 Removal efficiency (%)]]> <![CDATA[NO x Removal efficiency (%)]]> Recovery rate (%) 1 94 85 ~100 D-1 71 63 ~100 D-2 34 10 ~100 2 91 83 ~100 3 80 62 ~100 D-3 100 21 -
[0092] According to the data in Table 2 above, by comparing Example 1 with Comparative Example 1, it can be seen that compared with the commercially available ETS-10 molecular sieve used in Comparative Example 1, the Hg content of the catalyst prepared by using EVS-10 molecular sieve in Example 1 is 0 Removal efficiency and NO x The removal efficiency is better.
[0093] By comparing Example 1 with Comparative Example 2, it can be seen that although the product in Comparative Example 2 can also achieve a 100% recovery rate, its demercuration and denitrification efficiency is extremely low. The catalytic adsorbent prepared in Example 1 of the present disclosure has better synergistic demercuration and denitrification performance on the basis of 100% recovery.
[0094] Comparing Examples 1 to 3 of the present application with Comparative Example 3 (molecular sieve loaded silver), the catalytic adsorbent samples prepared in Examples 1 to 3 can simultaneously remove Hg 0 and NO x . And the recovery efficiency can reach 100%. Although comparative example 3 can achieve a good elemental mercury removal efficiency, the nitrogen oxide removal efficiency is extremely low, only 21%, and cannot be recovered by magnets. It shows that the catalytic adsorbent prepared by the method provided by the present disclosure has better synergistic mercury removal and denitrification performance and recovery performance.
[0095] Further comparison of Examples 1 to 3 shows that when the dispersing aid is added in Examples 1 to 2, the obtained catalytic adsorbent has a higher Hg 0 Removal efficiency and NO x Removal efficiency.
[0096] The preferred embodiments of the present disclosure are described in detail above, but the present disclosure is not limited to the specific details of the above embodiments, and within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all belong to the protection scope of the present disclosure.
[0097] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0098] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A catalytic adsorbent for flue gas demercuration and denitrification, It is characterized in that The catalytic adsorbent comprises a carrier, magnetic particles and active components; the magnetic particles comprise nano-Fe 3 O 4 Particles and coated with the nano-Fe 3 O 4 The silicon oxide layer on the surface of the particles, the active component is loaded on the carrier; the carrier includes EVS-10 molecular sieve, and the active component includes CeO 2 ; The catalytic adsorbent is prepared by a method comprising the following steps: (1) mixing a magnetic EVS-10 molecular sieve, a cerium source and water to obtain a raw material mixture, wherein the magnetic EVS-10 molecular sieve includes the carrier and the magnetic particles; (2) adding an alkaline solution to the raw material mixture for mixing, and then adding alcohol to obtain a colloidal precursor; (3) performing a first calcination treatment on the colloidal precursor; Wherein the magnetic EVS-10 molecular sieve comprises the EVS-10 molecular sieve and the magnetic particles; The mixing in step (1) further comprises adding a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride.
2. The catalytic adsorbent according to claim 1, It is characterized in that Based on the total weight of the catalytic adsorbent, the mass fraction of the magnetic particles is 5-50% by weight, the mass fraction of the carrier is 35-94% by weight, and the mass fraction of the active component is 1-15%.
3. The catalytic adsorbent according to claim 1, It is characterized in that The dispersing aid in step (1) is polymethacrylic acid.
4. The catalytic adsorbent according to claim 1, It is characterized in that In step (1), the weight ratio of the dispersing aid to the cerium source is (30-70): (10-20).
5. The catalytic adsorbent according to claim 1, It is characterized in that Step (1) also includes: ultrasonically treating the magnetic EVS-10 molecular sieve in water for 5 to 30 minutes, and then adding the cerium source and the dispersing aid to mix to obtain the raw material mixture.
6. The catalytic adsorbent according to claim 1, It is characterized in that The method also includes preparing the magnetic EVS-10 molecular sieve by the following steps: a. Put Fe 3 O 4 The particles, silicate solution and water are mixed, and then an acid is added to adjust the pH to obtain a first mixture; b. Keep the first mixture at 30-45° C. for 2-4 hours; then heat it to 85-95° C. and keep it for 1-2 hours; then cool it to 20-40° C.; perform a first separation using a magnetic separation device to obtain a first solid product having magnetic properties; c. Dispersing the EVS-10 molecular sieve and the first solid product in a solvent, performing a second separation to remove the solvent; and performing a second calcination treatment to obtain the magnetic EVS-10 molecular sieve.
7. The catalytic adsorbent according to claim 6, It is characterized in that In step a, an acid is added to adjust the pH to 9.3-9.7 to obtain the first mixture.
8. The catalytic adsorbent according to claim 6, It is characterized in that In step a, the Fe 3 O 4 The weight ratio of particles, silicate and water is (0.45~0.9):1:(27~54); The silicate comprises sodium silicate; the concentration of the silicate solution is 0.5-3 mol / L; The acid is hydrochloric acid or sulfuric acid; the concentration of the acid is 0.1-1 mol / L.
9. The catalytic adsorbent according to claim 6, It is characterized in that Step a comprises: 3 O 4 The particles and a suspension of deionized water are dispersed, wherein the dispersion method comprises at least one of ultrasonic treatment and mechanical stirring, and then the silicate solution is added to the obtained dispersion system.
10. The catalytic adsorbent according to claim 6, It is characterized in that In step c, the solvent is selected from one or more of toluene, acetone and ethyl acetate.
11. The catalytic adsorbent according to claim 10, It is characterized in that In step c, the solvent is toluene.
12. The catalytic adsorbent according to claim 6, It is characterized in that Step c comprises: adding the EVS-10 molecular sieve to the solvent for ultrasonic treatment, adding the first solid product and continuing ultrasonic treatment to obtain a suspension; and then performing a second separation; In step c, the conditions of the second calcination treatment include: a calcination temperature of 250-350° C. and a calcination time of 1-2 hours.
13. The catalytic adsorbent according to claim 12, It is characterized in that The second separation comprises: allowing the obtained suspension to stand for stratification, removing the upper layer solvent, and then evaporating at 90-110° C. to remove the residual solvent.
14. The catalytic adsorbent according to claim 1, It is characterized in that In step (1), the weight ratio of the magnetic EVS-10 molecular sieve, the cerium source and water is (90-5): (13-18): (50-60); The cerium source is a water-soluble cerium salt.
15. The catalytic adsorbent according to claim 14, It is characterized in that The cerium source is selected from one or more of cerium acetate, cerium chloride and cerium nitrate.
16. The catalytic adsorbent according to claim 1, It is characterized in that Step (2) comprises: mixing the raw material mixture and the alkaline solution and ultrasonically treating them for 5 to 30 minutes, and then adding alcohol to obtain the colloidal precursor; The alkaline solution comprises aqueous ammonia; and the alcohol comprises ethanol.
17. The catalytic adsorbent according to claim 16, It is characterized in that The volume ratio of the alkaline solution and the alcohol added is (4-8): (60-70).
18. The catalytic adsorbent according to claim 1, It is characterized in that In step (3), the conditions of the first calcination treatment include: in an inert atmosphere, a calcination temperature of 350-600° C., and a calcination time of 1-4 hours; wherein the inert atmosphere is nitrogen or argon; The method further comprises: before the first calcination treatment, subjecting the colloidal precursor to ultrasonic treatment for 5 to 30 minutes, and then evaporating to dryness at 70 to 100°C.
19. Use of the catalytic adsorbent according to any one of claims 1 to 18 in the field of flue gas demercurization and denitrification.
20. The use according to claim 19, It is characterized in that The flue gas is flue gas from a coal-fired power plant.
21. A method for treating flue gas from a coal-fired power plant, comprising contacting flue gas containing mercury and NOx generated by the coal-fired power plant with the catalytic adsorbent described in any one of claims 1 to 18, then passing the contacted flue gas through a magnetic separation device to separate the flue gas from the catalytic adsorbent, and the flue gas enters a subsequent treatment process to recycle the catalytic adsorbent.