Aluminum phosphate sol, slurry, catalytic cracking catalyst, preparation method and application thereof, and catalytic cracking method

A novel catalytic cracking catalyst was prepared by using a binder combining aluminum phosphate and organic acids. This solved the problems of equipment corrosion and environmental pollution in the traditional catalyst preparation process, improved catalytic performance and wear resistance, and is suitable for the cracking process of heavy oil.

CN116060119BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202111272528.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-11-12
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Existing catalytic cracking catalysts suffer from high chlorine content during preparation, leading to equipment corrosion and environmental pollution. Furthermore, traditional aluminum phosphate sols have insufficient binding and catalytic properties, making it difficult to meet the cracking requirements of heavy oil.

Method used

A novel catalytic cracking catalyst was prepared by using aluminum phosphate sol containing aluminum phosphate and organic acids as a binder, combined with silica sol. By controlling the pH value and composition ratio, the chlorine content of the binder was reduced, thereby improving the stability and catalytic performance of the catalyst.

Benefits of technology

This approach achieves improved catalyst efficiency, propylene selectivity, and wear resistance, while avoiding equipment corrosion and environmental pollution, and reducing manufacturing costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003329302010000221
    Figure BDA0003329302010000221
  • Figure BDA0003329302010000231
    Figure BDA0003329302010000231
Patent Text Reader

Abstract

The present invention relates to the field of catalytic cracking, and discloses an aluminum phosphate sol, a slurry, a catalytic cracking catalyst, a preparation method and application thereof, and a catalytic cracking method, wherein the aluminum phosphate sol comprises aluminum phosphate and an organic acid radical of a first organic acid, wherein the content of Al in the aluminum phosphate sol is 3-10 weight %; compared with 1 weight part of Al, the content of the organic acid radical of the first organic acid is 0.3-4 weight parts, and the content of the P element is 0.5-1.5 weight parts; the pH of the aluminum phosphate sol is 1-3. The aluminum phosphate sol contains an organic acid, which can increase the solid content of the slurry and reduce the viscosity of the slurry, and the catalytic performance and wear resistance of the prepared catalytic cracking catalyst are better than those of the catalyst prepared by the traditional aluminum phosphate sol, and the aluminum phosphate sol does not contain chlorine, so that the catalyst dechlorination process is simple, and the problem of the chlorine-containing sol binder is overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalytic cracking, and in particular to an aluminum phosphate sol, a preparation method of the aluminum phosphate sol, a slurry, a catalytic cracking catalyst and a preparation method and application thereof, and a catalytic cracking method. Background Art

[0002] Catalytic cracking has always been an important process technology for secondary processing of crude oil, and catalyst is one of its core technologies. Semi-synthetic catalytic cracking catalyst is to first synthesize molecular sieve catalytic material, then use kaolin as filler, molecular sieve as active component, various silicon / aluminum gel as binder, mix them, spray dry and prepare the catalyst. The semi-synthetic method has a simple preparation process, low preparation cost, and strong flexibility in formula adjustment. At present, it occupies a dominant position in the preparation process of catalytic cracking catalyst.

[0003] In the semi-synthetic process, the main function of the binder is to enable the catalyst to obtain the strength and particle size distribution required for industrial applications. As the catalytic cracking process processes heavier and inferior crude oil, it becomes increasingly important for the binder to be compatible with the filler and active components to provide the ability to crack heavy oil while providing good reaction selectivity.

[0004] The binders used in semi-synthetic catalysts mainly include aluminum binders (aluminum sol or peptized pseudo-boehmite), silicon-aluminum binders, double aluminum binders (aluminum sol + peptized pseudo-boehmite) and silicon binders (silica sol or silica gel).

[0005] The preparation method of FCC catalyst disclosed in USP4542118 uses aluminum hydroxychloride with better bonding performance as a binder to improve the anti-wear performance of the catalyst. However, since the FCC catalyst prepared by aluminum sol has low activity, the ability to crack macromolecules is limited. CN1098130A proposes a method for preparing FCC catalyst using a composite binder composed of aluminum sol and pseudo-boehmite, which can integrate the characteristics of peptized pseudo-boehmite with certain cracking activity and the advantages of aluminum sol with good bonding performance and less coke produced by the reaction product to improve the wear resistance, activity and selectivity of the catalyst to coke. When colloidal pseudo-boehmite and aluminum sol are used as binders for cracking catalysts, a large amount of hydrochloric acid gas will escape during the spray drying and molding process of the catalyst due to the high chlorine content, thereby corroding the equipment and causing environmental pollution; if the catalyst is not subjected to a dechlorination step after spray drying, the hydrochloric acid gas formed by the chlorine-containing catalyst in the presence of water vapor in the catalytic cracking unit will destroy the lattice of the molecular sieve in the cracking catalyst, significantly reducing the activity of the catalyst, and will also corrode the equipment and cause serious environmental pollution after entering the atmosphere.

[0006] In order to reduce the chlorine content in the catalyst using conventional aluminum sol as a binder, US Pat. No. 4,458,023 adds a calcination step after spray drying in the manufacturing process of molecular sieve cracking catalyst, so that the chlorine in the catalyst escapes in the form of hydrogen chloride. The disadvantage of this method is that hydrogen chloride has a serious corrosive effect on the calcination equipment and pollutes the surrounding environment.

[0007] US4542118 uses ammonia gas to contact the spray-dried catalyst for dechlorination of aluminum sol cracking catalyst, so that the hydrogen chloride therein reacts with ammonia to generate ammonium chloride, which is then washed away with water. This method still has the problems of equipment corrosion and environmental pollution during spray drying, and the operation is also relatively complicated. Summary of the invention

[0008] The purpose of the present invention is to provide a new aluminum phosphate sol, which contains organic acid, can increase the solid content of the slurry, reduce the viscosity of the slurry, and the catalytic performance and wear resistance of the prepared catalytic cracking catalyst are better than those of the catalyst prepared by the traditional aluminum phosphate sol. In addition, the aluminum phosphate sol does not contain chlorine, which makes the catalyst dechlorination process simple and overcomes the problem of chlorine-containing sol binder. The present invention also provides a catalyst containing the slurry, a preparation method and application thereof, and a catalytic cracking method.

[0009] In order to achieve the above object, the first aspect of the present invention provides an aluminum phosphate sol, wherein the aluminum phosphate sol comprises aluminum phosphate and an organic acid radical of a first organic acid, wherein the content of Al in the aluminum phosphate sol is 3-10 wt %;

[0010] Compared to 1 part by weight of Al, the content of the organic acid radical of the first organic acid is 0.3-4 parts by weight, and the content of the P element is 0.5-1.5 parts by weight;

[0011] The pH of the aluminum phosphate sol is 1-3.

[0012] The second aspect of the present invention provides a method for preparing the aluminum phosphate sol as described above, the method comprising: mixing an acid-soluble aluminum precursor with water to obtain a slurry with a solid content of 10-38 weight %; adding phosphoric acid and a first organic acid to the slurry for reaction to obtain an aluminum phosphate sol.

[0013] The third aspect of the present invention provides a slurry, which comprises, on a dry basis, 10-40 wt % of a molecular sieve, 20-45 wt % of a clay, and 15-40 wt % of a binder comprising an organic acid;

[0014] Wherein, the content of organic acid in the slurry is 1-10 wt % based on organic acid radical;

[0015] Wherein, the binder comprises aluminum phosphate sol;

[0016] Wherein, the pH of the slurry is 1.5-3.5.

[0017] Preferably, the molecular sieve is at least one selected from Y-type zeolite, Beta zeolite and a molecular sieve having an MFI structure.

[0018] More preferably, based on the dry weight of the molecular sieve, the molecular sieve comprises 1-99 wt % of the Y-type molecular sieve and 1-99 wt % of the molecular sieve having the MFI structure.

[0019] More preferably, based on the dry weight of the molecular sieve, the molecular sieve comprises 40-100 wt % of a molecular sieve having an MFI structure and 0-60 wt % of other molecular sieves selected from at least one of Beta zeolite and Y-type zeolite.

[0020] Preferably, the aluminum phosphate sol is the aluminum phosphate sol as described above.

[0021] Preferably, the binder further comprises silica sol; on a dry basis, the content of silica sol in the slurry is 2-30% by weight, and the content of aluminum phosphate sol is 2-20% by weight.

[0022] Preferably, the method for preparing the silica sol comprises: mixing and reacting a silicate with an inorganic acid and an alcohol solution of a second organic acid to obtain the silica sol.

[0023] Preferably, the temperature during the reaction is controlled not to exceed 45°C.

[0024] A fourth aspect of the present invention provides a catalyst, wherein the cracking catalyst is prepared from the slurry as described above.

[0025] A fifth aspect of the present invention provides a method for preparing a catalyst, which comprises molding and calcining the slurry as described above to obtain a cracking catalyst.

[0026] A sixth aspect of the present invention provides a catalyst prepared by the method described above.

[0027] A seventh aspect of the present invention provides use of the catalyst as described above in a catalytic cracking device.

[0028] An eighth aspect of the present invention provides a catalytic cracking method, which comprises: contacting hydrocarbon oil with a catalyst for reaction under catalytic cracking conditions; the catalyst is the catalyst as described above.

[0029] The aluminum phosphate sol of the present invention has very good stability and can be stored for a long time without affecting its bonding performance. The catalytic performance (such as cracking activity and propylene selectivity) and abrasion resistance of the catalytic cracking catalyst prepared by using the aluminum phosphate sol of the present invention are better than those of the catalyst prepared by the traditional aluminum phosphate sol.

[0030] In the present invention, the use of a binder containing an organic acid can greatly reduce the viscosity of the binder and the slurry, improve the fluidity of the material, thereby appropriately reducing the amount of binder used, reducing the catalyst manufacturing cost, and can increase the solid content of the slurry, thereby reducing the energy consumption of spray drying.

[0031] In the preferred embodiment of the present invention, a composite binder combining aluminum phosphate sol and silica sol is used, which can combine the characteristics of aluminum phosphate sol with good bonding properties, good catalyst strength, and certain cracking activity, and the advantage of silica sol in producing less coke in the catalyst reaction product, thereby further improving the catalyst's wear resistance, activity and selectivity for coke.

[0032] The preferred silica sol of the present invention has a longer stable existence time than the traditional silica sol. Under the preferred preparation method, the stable existence time of the silica sol can be further prolonged.

[0033] The binder of the present invention does not contain chlorine, and when using it to prepare a catalyst, chlorine will not be contained in the slurry before spray molding and the catalyst after spray molding, thereby avoiding equipment corrosion and environmental pollution. The binder has a low curing temperature and can be cured below 200°C (the curing temperature of chlorine-containing aluminum sol is generally greater than 300°C), so the temperature of the spray molding tail gas can be greatly reduced, thereby greatly reducing energy consumption and reducing the catalyst manufacturing cost.

[0034] In the present invention, when the preferred molecular sieve is used, more propylene can be produced and the selectivity of the catalyst for light olefins and coke can be improved. DETAILED DESCRIPTION

[0035] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0036] The first aspect of the present invention provides an aluminum phosphate sol, wherein the aluminum phosphate sol comprises aluminum phosphate and an organic acid radical of a first organic acid, wherein the content of Al in the aluminum phosphate sol is 3-10 wt %;

[0037] Compared to 1 part by weight of Al, the content of the organic acid radical of the first organic acid is 0.3-4 parts by weight, and the content of the P element is 0.5-1.5 parts by weight;

[0038] The pH of the aluminum phosphate sol is 1-3.

[0039] In the present invention, the Al content in the aluminum phosphate sol is 3-10 wt % (for example, it can be 3, 4, 5, 6, 7, 8, 9, 10 wt % and any range between any two values), preferably 5-7 wt %.

[0040] In the present invention, compared with 1 part by weight of Al, the content of P element is 0.5-1.5 parts by weight, for example, it can be 0.5, 0.7, 0.9, 1.1, 1.3, 1.5 parts by weight and any range between any two values, more preferably 0.8-1.2 parts by weight.

[0041] In the present invention, in the aluminum phosphate sol, compared with 1 weight part of Al, the content of the first organic acid is 0.3-4 weight parts (for example, it can be 0.3, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4 weight parts and any range between any two values), and more preferably 1-3 weight parts.

[0042] Preferably, the first organic acid is selected from at least one of oxalic acid, acetic acid, sulfosalicylic acid, citric acid and formic acid, more preferably oxalic acid and / or sulfosalicylic acid; in the preferred case, the cracking activity, propylene selectivity and abrasion resistance of the catalyst can be further improved.

[0043] In the present invention, the pH of the aluminum phosphate sol is 1-3 (for example, it can be 1, 1.5, 2, 2.5, 3 and any range between any two values); preferably, it is 1.5-2.

[0044] Preferably, the viscosity of the aluminum phosphate sol is 5-80 mPa·s; more preferably 20-60 mPa·s.

[0045] It should be understood that the aluminum phosphate sol also contains water.

[0046] The aluminum phosphate sol can be prepared in a conventional manner. Preferably, the preparation method of the aluminum phosphate sol is as shown in the second aspect.

[0047] A second aspect of the present invention provides a method for preparing the aluminum phosphate sol as described above, the method comprising: the method for preparing the aluminum phosphate sol comprises: mixing an acid-soluble aluminum precursor with water to obtain a slurry having a solid content of 10-38 wt % (for example, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38 wt % and any range between any two values); adding phosphoric acid and a first organic acid to the slurry for reaction to obtain an aluminum phosphate sol.

[0048] In the present invention, unless otherwise specified, solid content refers to the percentage of the weight of the remaining part of the slurry after drying to the total weight of the slurry. The drying method may be, for example, placing the slurry in an oven at 60-90° C. and drying to constant weight.

[0049] The catalyst prepared by using the preferred aluminum phosphate sol binder of the present invention can further improve the cracking activity, propylene selectivity and abrasion resistance of the catalyst compared with the catalyst prepared by using the aluminum phosphate sol binder prepared by the prior art.

[0050] Preferably, the acid-soluble aluminum precursor is selected from at least one of pseudo-boehmite, hydrated alumina with a diaspore structure, hydrated alumina with a gibbsite structure, hydrated alumina with a Bayerite structure, γ-alumina, η-alumina, θ-alumina and x-alumina; more preferably, pseudo-boehmite.

[0051] Preferably, the phosphoric acid is present in the form of a phosphoric acid solution.

[0052] Preferably, the phosphoric acid content in the phosphoric acid solution is 60-98 wt %, more preferably 70-90 wt %.

[0053] Preferably, the first organic acid exists in the form of a first organic acid solution.

[0054] Preferably, the content of the first organic acid in the first organic acid solution is 40-98 wt %, more preferably 40-70 wt %.

[0055] Preferably, the acid-soluble aluminum precursor is used in an amount such that the Al content in the aluminum phosphate sol is 3-10 wt %, preferably 5-7 wt %.

[0056] Preferably, the phosphoric acid is used in an amount such that the weight ratio of P to Al is 0.5-1.5, more preferably 0.8-1.2.

[0057] Preferably, the first organic acid is used in an amount such that the weight ratio of the organic acid to Al is 0.3-4 parts by weight, more preferably 1-3 parts by weight.

[0058] Preferably, the temperature during the reaction is controlled not to exceed 80°C, for example, it may not exceed 50, 55, 60, 65, 70, 75, 80°C or any range between any two values, more preferably not exceeding 65°C.

[0059] The third aspect of the present invention provides a slurry, which comprises, on a dry basis, 10-40 wt % of a molecular sieve, 20-45 wt % of a clay, and 15-40 wt % of a binder comprising an organic acid;

[0060] Wherein, the content of organic acid in the slurry is 1-10 wt % based on organic acid radical;

[0061] Wherein, the binder comprises aluminum phosphate sol;

[0062] Wherein, the pH of the slurry is 1.5-3.5.

[0063] In the present invention, on a dry basis, the slurry comprises 10-40 wt% of molecular sieve (for example, 10, 15, 20, 25, 30, 35, 40 wt% and any range between any two values), 20-45 wt% of clay (for example, 20, 25, 30, 35, 40, 45 wt% and any range between any two values), and 15-40 wt% of a binder comprising an organic acid (for example, 15, 20, 25, 30, 35, 40 wt% and any range between any two values). Preferably, on a dry basis, the slurry comprises 30-40 wt% of molecular sieve, 30-45 wt% of clay and 20-35 wt% of a binder comprising an organic acid.

[0064] In the present invention, the dry basis is processed according to the NB / SH / T 0953-2017 catalytic cracking catalyst ignition loss determination method. It should be understood that the content calculated on a dry basis means that the moisture and burnable components (such as organic matter) in the slurry are not counted.

[0065] In the present invention, the binder contains an organic acid, but the organic acid may not only come from the binder, but may also enter the slurry through exogenous addition or the like.

[0066] In the present invention, calculated as organic acid radicals, the content of organic acid in the slurry is 1-10 wt % (for example, it can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 wt % and any range between any two values). Preferably, calculated as organic acid radicals, the content of organic acid in the slurry is 4-8 wt %.

[0067] In the present invention, the organic acid radical is based on the total weight of the slurry and is calculated based on the theoretical value of various forms of organic acids present in the slurry.

[0068] In the present invention, the pH of the slurry is 1.5-3.5 (for example, it can be 1.5, 2, 2.5, 3, 3.5 and any range between any two values). Preferably, the pH of the slurry is 2-3.

[0069] Preferably, the viscosity of the slurry is 10000-200000 mPa·s.

[0070] The viscosity can be measured at 25° C. using a NDJ21 type rotational viscometer.

[0071] Preferably, the solid content of the slurry is 15-50% by weight, for example, it can be 15, 20, 25, 30, 35, 40, 45, 50% by weight and any range between any two values.

[0072] In the present invention, the molecular sieve is preferably a molecular sieve capable of catalyzing cracking reactions, and more preferably a zeolite molecular sieve and / or a non-zeolite molecular sieve.

[0073] The zeolite molecular sieve is preferably large-pore zeolite and / or medium-pore zeolite.

[0074] The large-pore zeolite is a zeolite with a pore structure of at least 0.7 nanometer ring openings, such as one or more of Y-type zeolite, faujasite, L zeolite, Beta zeolite, Ω zeolite, mordenite, and ZSM-18 zeolite, preferably Y-type zeolite and / or Beta zeolite.

[0075] The Y-type zeolite may be one or more of NaY-type zeolite, Y-type zeolite containing phosphorus and / or rare earth, ultrastable Y zeolite, and ultrastable Y zeolite containing phosphorus and / or rare earth.

[0076] Among them, the ultrastable Y zeolite can be, for example, a DASY series zeolite, including but not limited to DASY-0.0 molecular sieve and DASY-2.0 molecular sieve; the rare earth-containing ultrastable Y zeolite can be, for example, a SOY series molecular sieve, including but not limited to SOY-2, SOY-8 and SOY-12 molecular sieves.

[0077] The medium-pore zeolite is a zeolite with a pore structure having a ring opening greater than 0.56 nanometers and less than 0.7 nanometers, such as one or more of a molecular sieve with an MFI structure, ZSM-22 zeolite, ZSM-23 zeolite, ZSM-35 zeolite, ZSM-50 zeolite, ZSM-57 zeolite, MCM-22 zeolite, MCM-49 zeolite, and MCM-56 zeolite; preferably, a molecular sieve with an MFI structure.

[0078] A typical representative of the molecular sieve with MFI structure is ZSM-5 zeolite developed by Mobil Corporation of the United States, which has a ten-membered ring structure. Preferably, the molecular sieve with MFI structure is ZSM-5 molecular sieve and / or ZSM-5 molecular sieve modified with phosphorus or transition metal; preferably, the molecular sieve with MFI structure is at least one of ZSM-5, ZRP-1, ZRP-5, ZSP-2, ZSP-3 and ZSP-4.

[0079] The molar ratio of SiO2:Al2O3 of the molecular sieve with MFI structure is 15-100:1; preferably, the molar ratio of SiO2:Al2O3 of the molecular sieve with MFI structure is 20-60:1.

[0080] The non-zeolite molecular sieve refers to a molecular sieve in which the aluminum and / or silicon in the zeolite are partially or completely replaced by one or more of other elements such as phosphorus, titanium, gallium, and germanium, including one or more of silicates with different silicon-to-aluminum ratios (such as metal silicates, titanosilicates), metal aluminates, metal phosphates, aluminum phosphates, metal aluminum phosphates, and silicoaluminophosphates (such as SAPO molecular sieves).

[0081] Preferably, the molecular sieve is selected from at least one of Y-type zeolite, Beta zeolite and a molecular sieve having an MFI structure. More preferably, based on the dry weight of the molecular sieve, the molecular sieve comprises 1-99 wt% (for example, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 99 wt% and any range between any two values) of a Y-type molecular sieve and 1-99 wt% (for example, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 99 wt% and any range between any two values) of a molecular sieve having an MFI structure.

[0082] In a preferred embodiment of the present invention, based on the dry weight of the molecular sieve, the molecular sieve includes 40-100 wt%, such as 30-90 wt% or 30-60 wt% of a molecular sieve having an MFI structure and 0-60 wt%, such as 10-70 wt% or 40-70 wt% of other molecular sieves, wherein the other molecular sieves are preferably one or more of Beta zeolite and Y-type zeolite.

[0083] In a preferred embodiment of the present invention, the molecular sieve comprises a molecular sieve having an MFI structure and a Y-type zeolite containing a rare earth.

[0084] Preferably, the weight ratio of the molecular sieve having an MFI structure to the rare earth-containing Y-type zeolite is 1:0.1-5 (for example, it can be 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5 and any range between any two values).

[0085] In a specific embodiment of the present invention, the molecular sieve comprises ZSP-3 molecular sieve, DASY-2.0 molecular sieve and SOY-8 molecular sieve; on a dry basis, their weight ratio is 1: 0.05-3 (for example, it can be 0.05, 0.1, 0.5, 1, 1.5, 2, 2.5, 3 and any range between any two values): 0.05-2 (for example, it can be 0.05, 0.1, 0.5, 1, 1.5, 2 and any range between any two values).

[0086] Preferably, the clay is selected from at least one of kaolin, halloysite, montmorillonite, diatomaceous earth, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite; more preferably kaolin and / or halloysite.

[0087] In the present invention, the aluminum phosphate sol is preferably the aluminum phosphate sol described in the first aspect of the present invention.

[0088] In a preferred embodiment of the present invention, the binder further comprises silica sol. Preferably, on a dry basis, the content of silica sol in the slurry is 2-30 wt % (e.g., 2, 5, 10, 15, 20, 25, 30 wt % and any range between any two values), more preferably 5-20 wt %; the content of aluminum phosphate sol is 2-20 wt % (e.g., 2, 5, 10, 15, 20 wt % and any range between any two values), preferably 5-18 wt %.

[0089] In the present invention, the silica sol may be conventional silica sol in the art.

[0090] Preferably, the pH of the silica sol is 1-3 (for example, it can be 1, 1.5, 2, 2.5, 3 and any range between any two values); more preferably, it is 1.5-2.5.

[0091] Preferably, the viscosity of the silica sol is 0.2-50 mPa·s.

[0092] Preferably, the content of SiO2 in the silica sol is 1-15% by weight, for example, it can be 1, 3, 6, 9, 12, 15% by weight and any range between any two values, more preferably 5-11% by weight.

[0093] Preferably, the silica sol contains a second organic acid and an alcohol.

[0094] Preferably, in the silica sol, the content of the second organic acid is 1-15 wt % (for example, it can be 1, 3, 6, 9, 12, 15 wt % and any range between any two values), more preferably 4-12 wt %.

[0095] Preferably, the second organic acid is selected from at least one of oxalic acid, acetic acid, sulfosalicylic acid, citric acid and formic acid, more preferably oxalic acid and / or sulfosalicylic acid. In the preferred case, the propylene selectivity, coke selectivity and abrasion resistance of the catalyst can be further improved.

[0096] Preferably, in the silica sol, the content of the alcohol is 1-20 wt % (for example, 1, 5, 10, 15, 20 wt % and any range between any two values), more preferably 4-13 wt %.

[0097] The alcohol is preferably at least one selected from ethanol, propanol, ethylene glycol and glycerol.

[0098] The preparation method of the silica sol can be a conventional preparation method in the art, for example, silicate can be mixed with an inorganic acid and a second organic acid and reacted to obtain silica sol. Preferably, the preparation method of the silica sol comprises: mixing and reacting a silicate with an inorganic acid and an alcohol solution of a second organic acid to obtain silica sol. That is, the silica sol also contains an inorganic acid.

[0099] The silicate may be a conventional silicate in the art, such as sodium silicate, including but not limited to sodium water glass, etc.

[0100] Preferably, the temperature during the reaction is controlled not to exceed 45° C., more preferably not to exceed 35° C. In the preferred case, the properties of the silica sol can be further improved, thereby improving the coke selectivity and attrition resistance of the catalyst.

[0101] Preferably, the inorganic acid is selected from at least one of HCl, HNO3 and H2SO4, more preferably H2SO4.

[0102] Preferably, the inorganic acid is in the form of an inorganic acid solution, and the content of the inorganic acid in the inorganic acid solution is 5-40 wt % (for example, 5, 10, 15, 20, 25, 30, 35, 40 wt % and any range between any two values).

[0103] Preferably, the content of the second organic acid in the alcohol solution of the second organic acid is 30-80 wt % (eg, 30, 40, 50, 60, 70, 80 wt % and any range between any two values).

[0104] Preferably, the ratio of the inorganic acid to the second organic acid is 0.1-1:1 (for example, 0.1:1, 0.2:1, 0.4:1, 0.6:1, 0.8:1, 1:1 and any range between any two values) by weight.

[0105] It should be understood that the organic acid includes the first organic acid as described above and the second organic acid as described above.

[0106] The organic acid preferably comprises at least one of oxalic acid, sulfosalicylic acid, citric acid and formic acid, and more preferably oxalic acid and / or sulfosalicylic acid.

[0107] In the present invention, unless otherwise specified, the solvent used is water, which is preferably decationized water.

[0108] A fourth aspect of the present invention provides a catalyst, wherein the cracking catalyst is prepared from the slurry as described above.

[0109] Preferably, the catalyst has an apparent bulk density of 0.65-0.85 g / mL.

[0110] Preferably, the pore volume of the catalyst is 0.25-0.37 cm 3 / g.

[0111] Preferably, the catalyst has an attrition index of 0.5-3 wt% / h.

[0112] The above parameters can be evaluated by conventional methods in the art.

[0113] A fifth aspect of the present invention provides a method for preparing a catalytic cracking catalyst, the method comprising molding and calcining the slurry as described above to obtain a catalytic cracking catalyst.

[0114] Preferably, the forming method is spray drying, and the tail gas temperature is 170-190°C.

[0115] Preferably, the calcination conditions include: temperature of 400-600° C.; time of 1-10 h.

[0116] In a preferred embodiment of the present invention, the preparation method of the catalyst comprises sequentially adding clay, aluminum phosphate sol and molecular sieve into silica sol, mixing evenly to obtain a slurry; spray drying the slurry to obtain a microsphere catalyst; and drying and calcining the microsphere catalyst to obtain a catalyst product.

[0117] Preferably, the method further comprises, before drying the microsphere catalyst, aging the microsphere catalyst in water at a temperature of 60-70°C and a pH value of 4-6, filtering, washing with a 2-5 wt% ammonium sulfate solution at 60-70°C, filtering again, washing with water at 60-70°C, and adjusting the pH to 8-9 with aqueous ammonia after filtering.

[0118] In the present invention, clay and molecular sieve are preferably added in the form of clay powder and molecular sieve slurry, respectively, wherein the solid content of the molecular sieve slurry on a dry basis is preferably 30-40% by weight.

[0119] It should be understood that in order to obtain a product with good catalytic performance, the materials should be mixed as evenly as possible during the preparation process.

[0120] The mixing, washing and drying operations are conventional in the art and will not be described in detail here.

[0121] A sixth aspect of the present invention provides a catalytic cracking catalyst prepared by the method described above.

[0122] The performance of the catalyst is as described in the fourth aspect and will not be repeated here.

[0123] A seventh aspect of the present invention provides use of the catalytic cracking catalyst described above in catalytic cracking.

[0124] An eighth aspect of the present invention provides a catalytic cracking method, which comprises: contacting hydrocarbon oil with a catalyst for reaction under catalytic cracking conditions; the catalyst is the catalytic cracking catalyst as described above.

[0125] In the present invention, the hydrocarbon oil has a wide selection range and can be a conventional choice in the art, and the present invention will not be described in detail here.

[0126] The present invention has a wide range of reaction conditions for the catalytic cracking. Specifically, for example, the reaction conditions may include: a temperature of 400-650°C; a catalyst-oil ratio (weight) of 3-20; a material space velocity of 3-15h -1 .

[0127] In the present invention, preferably, the catalytic cracking method further comprises: hydrothermal aging the catalyst before the reaction. The present invention has a wide range of conditions for the hydrothermal aging. Preferably, the hydrothermal aging is carried out using 90%-100% water vapor. Further preferably, the hydrothermal aging conditions also include: a temperature of 700-900°C, preferably 750-850°C, and a time of 5-24h, preferably 10-18h.

[0128] The present invention will be described in detail below through examples.

[0129] In each embodiment and comparative example, the raw materials used to prepare the catalyst are as follows:

[0130] Pseudo-boehmite: produced by Shanxi Aluminum Plant, Al2O3 content 61% by weight, β-trihydrate Al2O3 <4% by weight;

[0131] Concentrated phosphoric acid: chemically pure, 85% by weight, produced by Beijing Chemical Plant;

[0132] ZSP-3 molecular sieve: produced by Qilu Branch of Catalyst Company, relative crystallinity>80%, SiO2 / Al2O3>40, Na2O<0.1 wt%.

[0133] DASY-2.0 molecular sieve: produced by Qilu Branch of Catalyst Company, with unit cell constant of 2.450nm, RE2O3 content of 2.10% by weight, and Na2O content of 1.25% by weight;

[0134] SOY-8 molecular sieve: produced by Qilu Catalyst Company, with a unit cell constant of 2.457nm, RE2O3 content of 7.30% by weight, and Na2O content of 1.12% by weight;

[0135] Halloysite: produced by China Kaolin Co., Ltd., quartz sand <1.5% by weight, Al2O3 37.1% by weight, Fe2O3 0.50% by weight, Na2O0.04% by weight, solid content on a dry basis of 74% by weight;

[0136] Sulfuric acid: chemically pure, concentration 98% by weight, produced by Beijing Chemical Plant;

[0137] Oxalic acid: chemically pure, colorless crystals or white powder, produced by Beijing Chemical Plant;

[0138] Citric acid: chemically pure, colorless crystals or white powder, produced by Beijing Chemical Plant;

[0139] Acetic acid: chemically pure, colorless crystalline hygroscopic solid, produced by Beijing Chemical Plant;

[0140] Ethanol: chemically pure, concentration of 95% by weight, produced by Beijing Chemical Plant;

[0141] Sodium water glass: contains SiO2 concentration of 26.3% by weight, modulus 3.2, produced by Catalyst Qilu Branch.

[0142] The properties of the crude oil are shown in Table 1:

[0143] Table 1

[0144] Crude oil Atmospheric residue <![CDATA[Density (20 °C), g·cm -3 > 0.8958 Carbon residue, weight % 3.37 <![CDATA[Viscosity, mm 2 ·S -1 > 100℃ 12.33 80℃ 20.67 Elemental composition, weight % C 86.41 H 12.93 S 0.13 N 0.27 Hydrocarbon composition, weight % Saturated hydrocarbons 65.6 Aromatics 19.6 Gel 12.8 Asphaltene 1.1 Metal content, ppm Fe 9.5 Ni 4.1 V 1.0 Na 0.9 Vacuum distillation range, ℃ Initial distillation point 286 10% 381 30% 431 50% 474 70% 542 90% 625

[0145] Chemical analysis and evaluation methods are as follows:

[0146] 1. Organic acid content is the theoretical value of organic acid weight content in slurry;

[0147] 2. For the determination of apparent bulk density and pore volume, refer to the RIPP test method;

[0148] 3. Determination of catalyst wear index: A certain amount of catalyst is placed in a wear index determination device and blown for 5 hours under a constant airflow. Except for the first hour, the weight percentage of fine powder less than 15 microns produced in the last four hours to the weight percentage of catalyst larger than 15 microns in the sample is called the catalyst wear rate, also known as the wear index, and the unit is weight %·h -1 .

[0149] The above analysis methods can be found in "Petrochemical Analysis Methods (RIPP Test Methods)" (edited by Yang Cuiding et al., Science Press, 1990).

[0150] The conversion rate refers to [(dry gas + liquefied gas + gasoline + coke) / fresh feedstock] × 100%; the liquid product yield refers to the sum of the yields of (liquefied gas + gasoline + diesel); propylene / liquefied gas refers to the weight content of propylene in liquefied gas.

[0151] The data given in the examples are all based on the weight percentage of each component in the solution.

[0152] Preparation Example 1

[0153] This preparation example is used to illustrate the preparation method of aluminum phosphate sol binder.

[0154] At room temperature (25°C), 4.92 kg of pseudo-boehmite (containing 3 kg of Al2O3) and 9.0 kg of decationized water were slurried for 30 minutes, and 6 kg of concentrated phosphoric acid was added to the slurry under stirring, and then 8 kg of oxalic acid solution (4 kg of oxalic acid + 4 kg of decationized water) was added, and the addition rate of concentrated phosphoric acid and oxalic acid was controlled so that the reaction temperature did not exceed 60°C. The reaction was continued with stirring for 40 minutes to obtain a colorless and transparent aluminum phosphate sol with a pH of 1.5.

[0155] The aluminum phosphate sol P-1 was analyzed to contain 6.21% by weight of P, 6.11% by weight of Al, P / Al (weight)=1.02, and 15.40% by weight of oxalic acid.

[0156] Preparation Example 2

[0157] This preparation example is used to illustrate the preparation method of aluminum phosphate sol binder.

[0158] At room temperature (25°C), 4.92 kg of pseudo-boehmite (containing 3 kg of Al2O3) and 9.0 kg of decationized water were slurried for 30 minutes, and 6 kg of concentrated phosphoric acid was added to the slurry under stirring, followed by 8 kg of acetic acid solution (6.5 kg of acetic acid + 1.5 kg of decationized water). The addition rate of concentrated phosphoric acid and acetic acid was controlled so that the reaction temperature did not exceed 60°C. The reaction was continued with stirring for 40 minutes to obtain a colorless and transparent aluminum phosphate sol with a pH of 1.6.

[0159] The aluminum phosphate sol P-2 was analyzed to contain 6.21% by weight of P, 6.11% by weight of Al, P / Al (weight)=1.02, and 25.03% by weight of acetic acid.

[0160] Preparation Example 3

[0161] This preparation example is used to illustrate the preparation method of aluminum phosphate sol binder.

[0162] The operation was carried out according to the method described in Preparation Example 1, except that the reaction temperature was controlled not to exceed 65°C, and the pH of the obtained aluminum phosphate sol was 1.5.

[0163] The aluminum phosphate sol P-1 was analyzed to contain 6.21% by weight of P, 6.11% by weight of Al, P / Al (weight)=1.02, and 15.40% by weight of oxalic acid.

[0164] Preparation Example 4

[0165] This preparation example is used to illustrate the preparation method of silica sol binder.

[0166] Take 0.86 kg of sulfuric acid, add 7.1 kg of decationized water to dilute, and after cooling, add 3 kg of oxalic acid-ethanol solution (1.46 kg of oxalic acid + 1.54 kg of ethanol). Take 5.9 kg of sodium water glass, add 8.0 kg of decationized water to dilute, and slowly add the diluted sodium water glass to the above sulfuric acid-oxalic acid dilute solution under stirring, control the addition rate of sodium water glass so that the temperature of the reaction system does not exceed 35°C, add 5.87% by weight of organic acid, and obtain silica sol S-1 with SiO2 concentration of 6.2% by weight and pH value of 1.9.

[0167] Preparation Example 5

[0168] This preparation example is used to illustrate the preparation method of silica sol binder.

[0169] Take 0.86 kg of sulfuric acid, add 7.1 kg of decationized water to dilute, cool to room temperature (25°C), and then add 3.0 kg of citric acid solution (1.46 kg of citric acid + 1.54 kg of ethanol). Take 5.9 kg of sodium water glass, add 8 kg of decationized water to dilute, and slowly add the diluted sodium water glass to the above sulfuric acid-citric acid dilute solution under stirring, and control the addition speed of the sodium water glass so that the temperature of the reaction system does not exceed 35°C to obtain silica sol S-2 with a SiO2 concentration of 6.2% by weight and a pH value of 2.4.

[0170] Preparation Example 6

[0171] This preparation example is used to illustrate the preparation method of silica sol binder.

[0172] The preparation was carried out according to the method described in Preparation Example 4, except that an equal mass of decationized water was used instead of ethanol to obtain silica sol S-3 with a SiO2 concentration of 6.2% by weight and a pH value of 2.2.

[0173] Comparative Preparation Example 1

[0174] This comparative preparation example is used to illustrate the preparation method of the silica sol binder.

[0175] The silica sol prepared according to the method described in CN1332754C is specifically prepared as follows: 0.63L sulfuric acid is diluted with 8.0kg decationized water and cooled. 7.61kg sodium water glass is diluted with 8.0kg decationized water and the diluted sodium water glass is slowly added to the above sulfuric acid dilute solution under stirring to obtain silica sol DS-1 with SiO2 concentration of 8.2% by weight and pH value of 2.5.

[0176] Comparative Preparation Example 2

[0177] This comparative preparation example is used to illustrate the preparation method of aluminum phosphate sol binder.

[0178] The aluminum phosphate sol was prepared according to the method described in CN102847547A, specifically by slurrying 0.66 kg of pseudo-boehmite (containing 0.40 kg of Al2O3) and 1.75 kg of decationized water for 30 minutes, slowly adding 2.6 kg of concentrated phosphoric acid (mass concentration 85%) to the slurry under stirring, heating to 70°C, and then reacting at this temperature for 45 minutes to obtain a colorless and transparent phosphorus-containing aluminum sol DP-1 with P / Al (weight) = 3.3 and pH = 2.46. The dry basis content was determined to be 42.95% by weight.

[0179] Example 1

[0180] This example is used to illustrate the preparation method of the catalyst described in the present invention.

[0181] According to the dosage described in Table 2, the catalyst was prepared as follows:

[0182] Add halloysite to the silica sol and stir for 1 hour to fully disperse the kaolin. Add aluminum phosphate sol and stir for 0.5 hour to prepare silicon-aluminum phosphate sol-clay slurry, then add ZSP-3 molecular sieve slurry (solid content of 36 weight % on a dry basis), DASY-2.0 molecular sieve slurry (solid content of 34 weight % on a dry basis) and SOY-8 molecular sieve slurry (solid content of 34 weight % on a dry basis) and stir for 0.5 hour to prepare sol-state catalyst slurry. The slurry is transported to a high-temperature spray tower by a high-pressure pump, sprayed and formed, and the tail gas temperature of the spray tower is controlled to be 180°C to obtain microspherical catalyst particles.

[0183] The microspherical catalyst particles were aged in decationized water at 70°C and a pH value of 4-5 for 1 hour, filtered, washed with a 5 wt% ammonium sulfate solution at 70°C for 10 minutes, filtered, and then washed with decationized water at 70°C for 10 minutes, and the pH value was adjusted to 8.0-9.0 with ammonia water. After filtering, drying at 150°C for 1 hour, and calcining at 500°C for 2 hours, catalysts AG were prepared respectively.

[0184] Example 2

[0185] This example is used to illustrate the preparation method of the catalyst described in the present invention.

[0186] According to the dosage described in Table 2, the catalyst was prepared as follows:

[0187] Add halloysite kaolin to decationized water for slurrying and stir for 1 hour to fully disperse the kaolin. Then add aluminum phosphate sol binder to prepare aluminum phosphate sol-clay slurry, then add ZSP-3 molecular sieve slurry, DASY-2.0 molecular sieve slurry and SOY-8 molecular sieve slurry, stir for 0.5 hour to prepare sol catalyst slurry. The slurry is transported to a high-temperature spray tower by a high-pressure pump, sprayed and formed, and the tail gas temperature of the spray tower is controlled to be 180°C to obtain microspherical catalyst particles.

[0188] The microspherical catalyst particles were calcined at 500°C for 2 hours, washed with a 3 wt% ammonium sulfate solution at 70°C for 10 minutes, filtered, and washed a second time with an ammonium sulfate solution of the same temperature and concentration, then washed a third time with decationized water at 70°C for 10 minutes, and adjusted the pH value to 8.0-9.0 with ammonia water, filtered, and dried at 150°C for 1 hour to prepare Catalyst H.

[0189] Comparative Example 1

[0190] This comparative example is used to illustrate the preparation method of a reference catalyst.

[0191] The method of Example 1 was followed, except that the aluminum phosphate sol binder prepared in Comparative Preparation Example 2 was used instead of the binder in Example 1. The amount used was shown in Table 2, and catalyst DB-1 was obtained.

[0192] The specific method for preparing the slurry is as follows: add halloysite to decationized water for slurrying, stir for 1 hour to fully disperse the kaolin, then add the aluminum phosphate sol binder prepared in Comparative Preparation Example 2 to prepare aluminum phosphate sol-clay slurry, then add ZSP-3 molecular sieve slurry, DASY-2.0 molecular sieve slurry and SOY-8 molecular sieve slurry, stir for 0.5 hour, and prepare a sol catalyst slurry.

[0193] The slurry is transported to a high-temperature spray tower by a high-pressure pump and sprayed into shape. The tail gas temperature of the spray tower is controlled at 180° C. to obtain microspherical catalyst particles.

[0194] The microspherical catalyst particles were calcined at 500°C for 2 hours, washed with a 3 wt% ammonium sulfate solution at 70°C for 10 minutes, filtered, and washed a second time with an ammonium sulfate solution of the same temperature and concentration, then washed a third time with decationized water at 70°C for 10 minutes, and adjusted the pH value to 8.0-9.0 with ammonia water, filtered, and dried at 150°C for 1 hour to prepare catalyst DB-1.

[0195] Comparative Example 2

[0196] This comparative example is used to illustrate the preparation method of a reference catalyst.

[0197] The method of Example 1 was followed, except that the silica sol prepared in Comparative Preparation Example 1 and the aluminum phosphate sol prepared in Comparative Preparation Example 2 were used as binders to replace the binder in Example 1. The amounts used were shown in Table 2, and catalyst DB-2 was obtained.

[0198] According to the dosage described in Table 2, the catalyst was prepared as follows:

[0199] Add decationized water and halloysite to the silica sol and stir for 1 hour to fully disperse the kaolin. Add aluminum phosphate sol and stir for 0.5 hour to prepare silicon-aluminum phosphate sol-clay slurry, then add ZSP-3 molecular sieve slurry, DASY-2.0 molecular sieve slurry and SOY-8 molecular sieve slurry and stir for 0.5 hour to prepare sol-state catalyst slurry. The slurry is transported to a high-temperature spray tower by a high-pressure pump and sprayed to form. The tail gas temperature of the spray tower is controlled to be 180°C to obtain microspherical catalyst particles.

[0200] The microspherical catalyst particles were aged in decationized water at 70°C and a pH value of 4.0-5.0 for 1 hour, filtered, washed with a 5 wt% ammonium sulfate solution at 70°C for 10 minutes, filtered, and washed with decationized water at 70°C for 10 minutes. The pH value was adjusted to 8.0-9.0 with ammonia water, filtered, dried at 150°C for 1 hour, and calcined at 500°C for 2 hours to prepare catalyst DB-2.

[0201] Test Case

[0202] 30 grams of the catalysts prepared in the above examples and comparative examples were taken and aged for 14 hours at 800°C and 100% steam atmosphere. The aged catalysts were then loaded into a reactor of a small fixed fluidized bed device and subjected to catalytic cracking reaction on the crude oil shown in Table 2. The reaction conditions included: reaction temperature of 520°C, reaction space velocity of 6h -1, the agent-oil weight ratio is 8.

[0203] The evaluation of the reaction products is shown in Table 3.

[0204]

[0205]

[0206] It can be seen from the data listed in Tables 2 and 3 that the wear index of catalyst A and catalyst C is better than that of catalyst B, indicating that when pseudo-boehmite is used as the aluminum source and a mixed acid of phosphoric acid and oxalic acid is used as the acidifier to prepare aluminum phosphate sol, the bonding performance of the aluminum phosphate sol is better than that of the aluminum phosphate sol prepared by phosphoric acid-acetic acid acidifier.

[0207] By comparing Catalyst A with Catalyst C, it can be seen that in the case of the preferred preparation method of aluminum phosphate sol, the wear resistance and catalytic performance of the prepared catalyst are better.

[0208] From the comparison between catalyst A and catalyst D, it can be seen that as the dosage of ZSP-3 molecular sieve increases, the cracking gas yield increases and the cracking performance of the catalyst is enhanced.

[0209] From the comparison between Catalyst A and Catalyst E, it can be seen that when the proportion of silica sol used increases, the wear resistance decreases, the coke yield decreases, and the coke selectivity of the catalyst increases.

[0210] The difference between Catalyst F and Catalyst A is that Catalyst A uses S-1 silica sol (using sulfuric acid-oxalic acid-ethanol solution), and Catalyst F uses S-2 silica sol (using sulfuric acid-citric acid-ethanol solution). The wear index of Catalyst A is lower than that of Catalyst F, indicating that the wear resistance of the catalyst prepared when using oxalic acid to prepare silica sol is better than that of citric acid.

[0211] The difference between Catalyst G and Catalyst A is that, when preparing the silica sol, Catalyst A uses a sulfuric acid-oxalic acid-ethanol solution, while Catalyst G uses a sulfuric acid-oxalic acid-water solution. The wear index of Catalyst A is lower than that of Catalyst G, indicating that the bonding performance of the silica sol prepared using ethanol is better than that of water.

[0212] The comparison shows that the wear index of catalysts DB-1 and DB-2 is higher than that of catalyst AH, indicating that the bonding performance of the binder containing organic acid provided by the present invention is better than that of the binder without organic acid. Moreover, the catalytic performance of the catalyst prepared by the technical solution of the present invention is also better than that of the catalyst prepared by the slurry without organic acid.

[0213] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An aluminum phosphate sol, characterized in that The aluminum phosphate sol comprises aluminum phosphate and an organic acid radical of a first organic acid, and the content of Al in the aluminum phosphate sol is 3-10% by weight; Compared to 1 part by weight of Al, the content of the organic acid radical of the first organic acid is 0.3-4 parts by weight, and the content of the P element is 0.5-1.5 parts by weight; The pH of the aluminum phosphate sol is 1-3; The preparation method of the aluminum phosphate sol comprises: mixing an acid-soluble aluminum precursor with water to obtain a slurry with a solid content of 10-38% by weight; adding phosphoric acid and a first organic acid to the slurry for reaction to obtain an aluminum phosphate sol; The first organic acid is oxalic acid and / or sulfosalicylic acid.

2. The aluminum phosphate sol according to claim 1, wherein In the aluminum phosphate sol, the content of Al is 5-7% by weight; and / or Compared to 1 part by weight of Al, the content of the organic acid radical of the first organic acid is 1-3 parts by weight, and the content of the P element is 0.8-1.2 parts by weight; and / or The pH of the aluminum phosphate sol is 1.5-2.

3. The aluminum phosphate sol according to claim 1 or 2, wherein The temperature is controlled not to exceed 80° C. during the reaction.

4. The aluminum phosphate sol according to claim 1 or 2, wherein The acid-soluble aluminum precursor is selected from at least one of pseudo-boehmite, hydrated alumina with a diaspore structure, hydrated alumina with a gibbsite structure, hydrated alumina with a bayerite structure, γ-alumina, η-alumina, θ-alumina and x-alumina.

5. The aluminum phosphate sol according to claim 4, wherein The acid-soluble aluminum precursor is pseudo-boehmite.

6. The aluminum phosphate sol according to claim 1 or 2, wherein The phosphoric acid exists in the form of a phosphoric acid solution, and the phosphoric acid content in the phosphoric acid solution is 60-98% by weight.

7. The aluminum phosphate sol according to claim 1 or 2, wherein The first organic acid exists in the form of a first organic acid solution, and the content of the first organic acid in the first organic acid solution is 40-98% by weight.

8. A slurry, characterized in that: On a dry basis, the slurry comprises 10-40 wt % of a molecular sieve, 20-45 wt % of a clay, and 15-40 wt % of a binder comprising an organic acid; Wherein, the content of organic acid in the slurry is 1-10% by weight, calculated as organic acid radical; Wherein, the binder contains aluminum phosphate sol; the aluminum phosphate sol is the aluminum phosphate sol according to any one of claims 1 to 7; Wherein, the pH of the slurry is 1.5-3.

5.

9. The slurry according to claim 8, wherein The slurry comprises, on a dry basis, 30-40 wt % of molecular sieve, 30-45 wt % of clay, and 20-35 wt % of a binder comprising an organic acid.

10. The slurry according to claim 8, wherein Calculated as organic acid radical, the content of organic acid in the slurry is 4-8% by weight.

11. The slurry according to claim 8, wherein The pH of the slurry is 2-3.

12. The slurry according to claim 8, wherein The solid content of the slurry is 15-50% by weight.

13. The slurry according to claim 8, wherein The molecular sieve is a molecular sieve capable of catalyzing cracking reactions.

14. The slurry according to claim 13, wherein The molecular sieve is a zeolite molecular sieve and / or a non-zeolite molecular sieve.

15. The slurry according to claim 14, wherein The molecular sieve is at least one selected from Y-type zeolite, Beta zeolite and a molecular sieve having an MFI structure.

16. The slurry according to claim 15, wherein Based on the dry weight of the molecular sieve, the molecular sieve comprises 1-99 wt % of a Y-type molecular sieve and 1-99 wt % of a molecular sieve having an MFI structure; and / or Based on the dry weight of the molecular sieve, the molecular sieve comprises 40-100 wt % of a molecular sieve having an MFI structure and 0-60 wt % of other molecular sieves selected from at least one of Beta zeolite and Y-type zeolite.

17. The slurry according to claim 8, wherein The clay is selected from at least one of kaolin, halloysite, montmorillonite, diatomaceous earth, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite.

18. The slurry according to claim 17, wherein The clay is kaolin and / or halloysite.

19. The slurry according to claim 8, wherein The binder further comprises silica sol; on a dry basis, the content of silica sol in the slurry is 2-30% by weight, and the content of aluminum phosphate sol is 2-20% by weight.

20. The slurry according to claim 19, wherein On a dry basis, the content of the silica sol in the slurry is 5-20% by weight, and the content of the aluminum phosphate sol is 5-18% by weight.

21. The slurry according to claim 19, wherein The pH of the silica sol is 1-3.

22. The slurry according to claim 21, wherein The pH of the silica sol is 1.5-2.

5.

23. The slurry according to claim 19, wherein In the silica sol, the content of SiO2 is 1-15% by weight.

24. The slurry according to claim 19, wherein The silica sol comprises a second organic acid and an alcohol; In the silica sol, the content of the second organic acid is 1-15% by weight, and the content of the alcohol is 1-20% by weight.

25. The slurry according to claim 24, wherein The second organic acid is selected from at least one of oxalic acid, acetic acid, sulfosalicylic acid, citric acid and formic acid.

26. The slurry according to claim 25, wherein The second organic acid is oxalic acid and / or sulfosalicylic acid.

27. The slurry according to claim 24, wherein The alcohol is selected from at least one of ethanol, propanol, ethylene glycol and glycerol.

28. The slurry according to claim 24, wherein The preparation method of the silica sol comprises: mixing and reacting silicate with an inorganic acid and an alcohol solution of a second organic acid to obtain the silica sol.

29. The slurry according to claim 28, wherein The temperature is controlled not to exceed 45°C during the reaction.

30. The slurry according to claim 28, wherein The inorganic acid is selected from at least one of HCl, HNO3 and H2SO4.

31. The slurry according to claim 30, wherein The inorganic acid is H2SO4.

32. The slurry according to claim 28, wherein The inorganic acid exists in the form of an inorganic acid solution, and the content of the inorganic acid in the inorganic acid solution is 5-40 weight %.

33. The slurry according to claim 28, wherein The content of the second organic acid in the alcohol solution of the second organic acid is 30-80% by weight.

34. The slurry according to claim 28, wherein The inorganic acid and the second organic acid are used in a ratio of 0.1-1:1 by weight.

35. The slurry according to claim 24, wherein The organic acid includes a first organic acid and a second organic acid.

36. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst is prepared from the slurry described in any one of claims 8-35.

37. A method for preparing a catalytic cracking catalyst, characterized in that: The method comprises molding and calcining the slurry described in any one of claims 8 to 35 to obtain a catalytic cracking catalyst.

38. The method of claim 37, wherein: The molding method is spray drying, and the tail gas temperature is 130-200°C.

39. The method of claim 38, wherein: The exhaust gas temperature is 170-190℃.

40. The method of claim 37, wherein: The calcination conditions include: temperature of 400-600° C. and time of 1-10 h.

41. A catalytic cracking catalyst prepared by the method according to any one of claims 37 to 40.

42. Use of the catalytic cracking catalyst according to claim 36 or 41 in catalytic cracking.

43. A method for catalytic cracking, characterized in that: The method comprises: contacting hydrocarbon oil with a catalyst for reaction under catalytic cracking conditions; the catalytic cracking catalyst is the catalytic cracking catalyst according to claim 36 or 41.

Citation Information

Patent Citations

  • Inorganic binder containing phosphorus and aluminum compounds

    CN102847547A

  • Cracking catalyst and preparing process thereof

    CN1098130A

  • Cracking catalyst using silicon adhesive and its use

    CN1332754C

  • Catalyst manufacture

    US4458023A

  • Catalyst manufacture

    US4542118A