Indium tin oxide material and preparation method and application thereof

By reducing the tin content in indium tin oxide materials and doping elements such as Hf to improve their density, the problems of low ITO target density and high carrier concentration are solved, and TCO film preparation with high transmittance and mobility are achieved , improving the efficiency and production stability of photovoltaic cells.

CN116072326BActive Publication Date: 2024-11-12ZHONGSHAN ZL ADVANCED MATERIALS TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310075230.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-07
Publication Date
2024-11-12
Estimated Expiration
2043-02-07

AI Technical Summary

Technical Problem

The indium tin oxide target (ITO target) used in existing photovoltaic HJT batteries has a high carrier concentration due to the high doping concentration, which leads to a greater parasitic absorption of long-band light by the TCO film, which limits the improvement of battery efficiency. Low sintering activity leads to low density and poor production stability.

Method used

Develop an indium tin oxide material with a low tin content (≤1%). It improves the density and density of the material by doping Hf and other elements (such as Ti, Zr, Ce, Ga), and is prepared by specific preparation methods. High-density ITO targets are obtained for sputtering coating to prepare TCO films, reducing carrier concentration to improve transmittance and mobility.

Benefits of technology

The high transmittance (90.0-90.5%) and high mobility (80.5-82.5cm2/V.S) of TCO films under low concentration carrier conditions are achieved, which improves the short-circuit current and conversion efficiency of photovoltaic cells, and is suitable for Photovoltaic heterojunction battery field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004065863540000071
    Figure BDA0004065863540000071
  • Figure BDA0004065863540000081
    Figure BDA0004065863540000081
  • Figure BDA0004065863540000082
    Figure BDA0004065863540000082
Patent Text Reader

Abstract

The invention belongs to the technical field of photovoltaic cells, and provides an indium tin oxide material and a preparation method and application thereof. The indium tin oxide material provided by the invention comprises indium oxide, tin oxide, hafnium oxide and oxide of X in a specific ratio, wherein X is one or more of Ti, Zr, Ce and Ga, and the mass content of tin oxide in the metal oxide component of the invention is ≤1%, and Hf and X elements are doped. The density of the indium tin oxide material is 7.0-7.08 g / m 3 , the density is improved, and the indium tin oxide material can be further used to deposit TCO thin films, which increases the transmittance of long-wavelength light (the transmittance between 400-1200nm reaches 90.0-90.5%) and is (1.43-1.52)×10 20 cm ‑3 Under low concentration carrier doping, 80.5-82.5cm 2 The higher mobility of / VS can be well applied in the field of photovoltaic heterojunction cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic cells, and more specifically, to an indium tin oxide material and a preparation method and application thereof. Background Art

[0002] In the preparation process of crystalline silicon heterojunction solar cells (HJT), doped amorphous silicon thin films and intrinsic amorphous silicon thin films are usually deposited on both sides of the silicon wafer to form a heterojunction structure with the crystalline silicon substrate, change the bandgap width, and thus obtain a high open circuit voltage. The lateral electronic conductivity of the doped amorphous silicon film is poor, and it needs to be covered with a transparent conductive oxide film (i.e., TCO film) for light transmission and current transmission.

[0003] TCO thin film is deposited on the substrate surface by physical vapor deposition (PVD) or reactive plasma deposition (RPD). PVD is the mainstream method for preparing TCO thin film in the industry. Its basic principle is to ionize the process gas Ar into Ar under the action of electric and magnetic fields. + Plasma, accelerated high-energy particles (Ar + ) obtains high energy and bombards the target material. The atoms on the surface of the target material break away from the original lattice and escape. The sputtered particles are deposited on the substrate surface and react with oxygen atoms to form oxides. The coating principle of RPD is that Ar gas generates plasma through a plasma gun, enters the process chamber, and then guides the Ar plasma to hit the target material through a magnetic field. The target material sublimates and deposits on the substrate. Both deposition methods require the use of target materials. Due to the differences in deposition principles, the material performance requirements for the target material are different.

[0004] Since the absorption of TCO film is related to the free carrier concentration in the film, reducing the free carrier concentration can effectively reduce its long-wave parasitic absorption. The low-doping concentration TCO film on the positive surface (light-receiving surface) of the HJT cell reduces the optical parasitic absorption and has a high long-wave transmittance, which can effectively increase the short-circuit current of the cell, thereby improving the cell efficiency.

[0005] In the full wavelength range of sunlight (300-2500nm), the energy in the visible light range (400-760nm) accounts for 43%, the energy in the ultraviolet region (300-400nm) accounts for 5%, and the energy in the near-infrared region (760-2500nm) accounts for 52% of the total energy. TCO film has different optical properties in different light bands, mainly including ultraviolet cutoff characteristics (intrinsic absorption), transparency in the visible light band, and reflectivity in the near and mid-infrared bands.

[0006] The indium tin oxide target (ITO target) used in the existing photovoltaic HJT cells is mainly composed of indium oxide and tin oxide. The mass ratio of indium oxide to tin oxide is usually 90:10 or 97:3. While the high doping concentration of tin oxide brings high conductivity, the TCO film has a high absorption of light itself and a low transmittance of long-wavelength light (86-88%, @400-1200nm), which makes it impossible to maximize the use of sunlight, which also seriously restricts the improvement of HJT cell efficiency. Reducing the doping content of tin oxide in the ITO target can effectively reduce the carrier concentration of the film and reduce the parasitic absorption of long-wavelength light by the TCO film.

[0007] Due to the low sintering activity of indium oxide materials, single-component indium oxide is difficult to sinter and has a low density. Doped tin oxide can be used as a sintering aid to effectively increase the sintering density, but the density of the sintered ITO target material usually decreases with the decrease of tin content. When low-density ITO targets are used for sputtering coating, they usually cause abnormalities such as nodules and cracking, which seriously affect the stable production on site. Therefore, it is urgent to develop a high-density, low-tin content ITO target material for sputtering coating to produce TCO thin films, which can improve the transmittance and obtain higher mobility at low carrier concentrations. Summary of the invention

[0008] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an indium tin oxide material and a preparation method and application thereof. The indium tin oxide material provided by the present invention has a low tin content (the mass percentage of tin oxide in the metal oxide component is ≤1%), improves the density, and has a high density (7.0-7.08g / m 3 ), and further used as ITO target for sputtering coating, the TCO film produced has high transmittance (the transmittance between 400-1200nm reaches 90.0-90.5%), and the transmittance between (1.43-1.52)×10 20 cm -3 Under low concentration carrier doping, a higher mobility (80.5-82.5cm 2 / VS).

[0009] A first aspect of the present invention provides an indium tin oxide material.

[0010] Specifically, an indium tin oxide material includes a metal oxide component, and the metal oxide component includes the following components in terms of mass percentage:

[0011] Indium oxide 95-99.5%, tin oxide 0.1-1%, hafnium oxide 0.1-0.5%, X oxide 0.1-0.5%, wherein X is one or more of Ti, Zr, Ce and Ga.

[0012] The indium tin oxide material provided by the present invention comprises indium oxide, tin oxide, hafnium oxide and oxide of X in a specific ratio, wherein X is one or more of Ti, Zr, Ce and Ga. The present invention reduces the tin content (the mass of the tin oxide of the present invention is ≤ 1% of the total mass of the metal oxide component) on the basis of the traditional indium tin oxide target material, and by doping Hf element and X element, Hf exists in the form of +4 valence, and the ion radius is close to In 3+ ions, which can achieve In 3+ The replacement of ions improves the mobility of TCO films deposited at low temperatures (150-200°C); and the density of the target material is increased by doping with the X element, so that it can be well applied in the field of photovoltaic heterojunction cells.

[0013] Further preferably, the metal oxide component comprises the following components in terms of mass percentage:

[0014] Indium oxide 96-99%, tin oxide 0.1-0.8%, hafnium oxide 0.1-0.3%, X oxide 0.1-0.3%.

[0015] More preferably, the metal oxide component comprises the following components in terms of mass percentage:

[0016] Indium oxide 98-99%, tin oxide 0.5-0.8%, hafnium oxide 0.25-0.3%, X oxide 0.25-0.3%.

[0017] Preferably, the indium oxide is indium oxide powder.

[0018] Preferably, the tin oxide is tin oxide powder.

[0019] Preferably, the hafnium oxide is hafnium oxide powder.

[0020] Preferably, the specific surface area of ​​the indium oxide powder is 6-20 m 2 / g.

[0021] Preferably, the specific surface area of ​​the tin oxide powder is 10-25m 2 / g.

[0022] Preferably, the oxide of X is X oxide powder.

[0023] Preferably, the indium tin oxide material further includes a binder and / or a plasticizer.

[0024] Preferably, the mass of the binder is 0.4-2.5% of the total mass of the metal oxide component.

[0025] Preferably, the mass of the plasticizer is 0.1-2% of the total mass of the metal oxide component.

[0026] Preferably, the binder is polyvinyl alcohol (PVA).

[0027] Preferably, the plasticizer is polyethylene glycol (PEG).

[0028] Preferably, the density of the indium tin oxide material is 7.0-7.08 g / m 3 (The density is measured using the Archimedes displacement method).

[0029] Further preferably, the density of the indium tin oxide material is 7.03-7.08 g / m 3 .

[0030] A second aspect of the present invention provides a method for preparing an indium tin oxide material.

[0031] A method for preparing an indium tin oxide material comprises the following steps:

[0032] The components are mixed, molded, degreased and sintered to obtain the indium tin oxide material.

[0033] Preferably, the mixing of the components further includes ball milling.

[0034] Preferably, after the ball milling, a binder and / or a plasticizer is added and mixed, and then drying is performed.

[0035] Preferably, the drying is spray drying.

[0036] Preferably, the specific surface area of ​​the powder obtained after spray drying is 5-25m 2 / g.

[0037] Preferably, the powder obtained after spray drying has a bulk density of 1.20-1.65 g / cm 3 .

[0038] Preferably, the molding pressure is 100-200 MPa.

[0039] Preferably, the sintering temperature is 1500-1650° C., and the sintering time is 72-120 h.

[0040] Preferably, the sintering atmosphere is an oxygen atmosphere and / or a nitrogen atmosphere.

[0041] Preferably, the method for preparing indium oxide comprises the following steps:

[0042] Dissolve metallic indium in an acid solution to generate an indium trichloride solution, then add an alkaline solution to generate a precipitate, age for 6-7 hours, filter, and dry to obtain indium hydroxide, which is then calcined at high temperature to obtain indium oxide.

[0043] Preferably, the acid solution is hydrochloric acid.

[0044] Preferably, the alkaline solution is aqueous ammonia.

[0045] Preferably, the temperature of the high-temperature calcination is 600-1000° C., and the time of the high-temperature calcination is 8-12 hours.

[0046] Preferably, the tin oxide is prepared by a chemical precipitation method.

[0047] A third aspect of the present invention provides an application of an indium tin oxide material.

[0048] An application of indium tin oxide material in the field of photovoltaic cells.

[0049] A target material for a photovoltaic cell comprises the indium tin oxide material.

[0050] Preferably, the photovoltaic cell is a photovoltaic heterojunction cell.

[0051] A transparent conductive oxide film is made of the indium tin oxide material.

[0052] Preferably, the mobility of the transparent conductive oxide film is 80.5-81.5 cm 2 / VS.

[0053] Preferably, the carrier concentration of the transparent conductive oxide film is 1.43×10 20 cm -3 .

[0054] Preferably, the light transmittance of the transparent conductive oxide film is 90-90.5%.

[0055] A method for preparing a transparent conductive oxide film comprises the following steps:

[0056] The indium tin oxide material is deposited on a substrate to prepare a transparent conductive oxide film (TCO film).

[0057] Preferably, the deposition is performed by sputtering. The target material developed by the present invention is mainly used for sputtering (PVD).

[0058] Preferably, the sputtering coating has a coating power of 1.0-10.0 kW.

[0059] Preferably, the temperature of the sputtering coating is 150-200°C.

[0060] Preferably, the substrate is a glass substrate.

[0061] Preferably, the deposited film has a thickness of 70-90 mm.

[0062] Further preferably, the deposited film thickness is 80-90 mm.

[0063] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0064] (1) The indium tin oxide material provided by the present invention comprises indium oxide, tin oxide, hafnium oxide and oxide of X in a specific ratio, wherein X is one or more of Ti, Zr, Ce and Ga. The present invention reduces the tin content (the mass of the tin oxide of the present invention is ≤ 1% of the total mass of the metal oxide components), and dopes Hf and X elements to increase the density of the indium tin oxide material (7.0-7.08 g / m 3 ), the indium tin oxide material can be further used to deposit TCO thin films, which increases the transmittance of long-wavelength light (the transmittance between 400-1200nm reaches 90.0-90.5%), and the transmittance between (1.43-1.52)×10 20 cm -3 Under low concentration carrier doping, a higher mobility (80.5-82.5cm 2 / VS), which can increase the short-circuit current of heterojunction batteries, thereby improving battery conversion efficiency, and is well applied in the field of photovoltaic heterojunction batteries;

[0065] (2) The present invention mixes the components, dries, shapes, degreases, and sinters to obtain the indium tin oxide material. The preparation method of the present invention is simple and easy to operate. DETAILED DESCRIPTION

[0066] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0067] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0068] Example 1

[0069] An indium tin oxide material comprises a metal oxide component, a binder and a plasticizer, wherein the metal oxide component comprises the following components in terms of mass percentage:

[0070] Indium oxide powder 99%, tin oxide powder 0.5%, hafnium oxide powder 0.25%, titanium oxide powder 0.15%, gallium oxide powder 0.1%; the mass of the binder (PVA) is 2% of the mass of the indium tin oxide material, and the mass of the plasticizer (PEG) is 1% of the mass of the indium tin oxide material.

[0071] The method for preparing the above-mentioned indium tin oxide material comprises the following steps:

[0072] (1) Preparation of indium oxide powder:

[0073] The indium ingot (4N5) was dissolved in dilute hydrochloric acid to generate an indium trichloride solution. The solution was heated and a slightly excessive amount of ammonia water was added to generate a precipitate, which was heated and matured together with the mother liquor for 6.5 hours; the precipitate was filtered and washed until there was no chloride ion, and dried at room temperature to obtain indium hydroxide; the indium hydroxide was calcined at 1000°C in an air atmosphere for 8 hours to form indium oxide powder, and the specific surface area of ​​the powder was measured to be 8.8m 2 / g.

[0074] (2) Preparation of tin oxide powder:

[0075] Sodium carbonate solution was added to sodium stannate solution, stirred in a mixer, washed and dried to obtain nano SnO2 powder. The specific surface area of ​​the powder was 15m 2 / g.

[0076] (3) Preparation of indium tin oxide powder:

[0077] After mixing the components of the metal oxide components, ball milling was performed. The ball milling used 0.65 mm and 0.30 mm zirconium beads in turn, and a binder (PVA) and a plasticizer (PEG) were added. After spray drying, the powder had a specific surface area of ​​10.5 m 2 / g, its bulk density is 1.35g / cm 3 .

[0078] (4) Embryo forming:

[0079] Use a rotating target mold to inject powder into the mold, use a wet hydraulic press, and use a molding pressure of 280MPa to obtain a target blank after static pressure strengthening.

[0080] (5) Degreasing and sintering:

[0081] In a normal pressure air atmosphere, the target blank is kept at 450°C for 10 hours for degreasing, and then sintered at a high temperature in an oxygen atmosphere with a maximum sintering temperature of 1560°C to obtain an indium tin oxide material.

[0082] Embodiment 2-4

[0083] The difference between the indium tin oxide materials of Examples 2-4 and Example 1 lies in the different components and contents of the metal oxide components, as shown in Table 1.

[0084] Table 1 Components and mass percentages of metal oxide components in each embodiment

[0085] Example 1 Example 2 Example 3 Example 4 Indium oxide powder 99 99 99 99 Tin oxide powder 0.5 0.5 0.5 0.5 Hafnium Oxide Powder 0.25 0.25 0.25 0.25 Titanium oxide powder 0.15 0 0.25 0 Gallium oxide powder 0.1 0 0 0 Zirconia powder 0 0.15 0 0.25 Cerium oxide powder 0 0.1 0 0

[0086] Comparative Examples 1-5

[0087] The difference between Comparative Examples 1-5 and Example 1 is that the components and contents of the metal oxide components are different, as shown in Table 2 below.

[0088] Table 2 Metal oxide components and their mass percentages of each comparative example

[0089] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Indium oxide powder 99 99 99 98 98 Tin oxide powder 1 0.5 0.5 0.5 0.5 Hafnium Oxide Powder 0 0.5 0 0.5 1 Titanium oxide powder 0 0 0.5 1 0.5

[0090] Application Example 1

[0091] Preparation of ITO target material: The indium tin oxide material prepared in the above-mentioned embodiments and comparative examples is the ITO target material.

[0092] Application Example 2

[0093] Preparation of TCO thin film: On a cleaned glass substrate, the ITO target materials prepared in the above embodiments and comparative examples were used to prepare TCO thin films by sputtering deposition.

[0094] Product effect testing

[0095] 1. Binding flaw detection

[0096] The ITO target (rotating target) prepared in the above-mentioned embodiments and comparative examples was coated with indium and bound to a titanium tube, and ultrasonic flaw detection was performed to find no dark cracks, and then subsequent sputtering deposition was performed to prepare a TCO film.

[0097] 2. Density of ITO material

[0098] Table 3 Density of indium tin oxide materials obtained in various embodiments and comparative examples

[0099]

[0100]

[0101] 3. TCO film coating process parameters and performance testing

[0102] Table 4 Coating process parameters and performance test results of TCO films prepared in various embodiments and comparative examples

[0103]

[0104] It can be seen from Table 3 and Table 4 that the mass content of tin oxide in the metal oxide component of the ITO target prepared in Examples 1-4 of the present invention is ≤1%, and the target density reaches 7.0-7.08 g / m 3The ITO targets prepared in Examples 1 to 4 of the present invention were used to sputter and deposit TCO thin films. The transmittance between 400 and 1200 nm reached 90.0-90.5%, and the transmittance between (1.43-1.52)×10 20 cm -3 At lower carrier concentrations, the mobility of the film reaches 80.5-82.5 cm 2 / VS, indicating that the ITO target prepared by the present invention has the characteristics of low tin doping content and high density, and the prepared TCO film has high mobility and high transmittance at a lower carrier concentration. However, the target density of comparative examples 1-5 is low, and the mobility and transmittance of the prepared TCO film are both reduced.

Claims

1. An indium tin oxide material, characterized in that: The invention comprises a metal oxide component, wherein the metal oxide component comprises the following components in terms of mass percentage: Indium oxide 95-99.5%, tin oxide 0.1-1%, hafnium oxide 0.1-0.5%, X oxide 0.1-0.5%, wherein X is one or more of Ti, Zr, Ce, and Ga; The sum of the above components is 100%; The TCO film made of the indium tin oxide material has a light transmittance of 90.0-90.5% between 400-1200 nm and a light transmittance of 90.0-90.5% between (1.43-1.52)×10 20 cm -3 The mobility under low concentration carrier doping is 80.5-82.5cm 2 / V·S.

2. The indium tin oxide material according to claim 1, characterized in that: The metal oxide component comprises the following components in terms of mass percentage: Indium oxide 96-99%, tin oxide 0.1-0.8%, hafnium oxide 0.1-0.3%, X oxide 0.1-0.3%.

3. The indium tin oxide material according to claim 1, characterized in that: The indium tin oxide material also includes a binder and / or a plasticizer.

4. The indium tin oxide material according to claim 1, characterized in that: The density of the indium tin oxide material is 7.0-7.08 g / m 3 .

5. The method for preparing the indium tin oxide material according to any one of claims 1 to 4, characterized in that: The steps include: The components are mixed, molded, degreased and sintered to obtain the indium tin oxide material.

6. The preparation method according to claim 5, characterized in that: The sintering temperature is 1500-1650° C., and the sintering time is 72-120 hours.

7. Use of the indium tin oxide material according to any one of claims 1 to 4 in the field of photovoltaic cells.

8. A target material for a photovoltaic cell, characterized in that: The invention comprises the indium tin oxide material according to any one of claims 1 to 4.

9. A transparent conductive oxide film, characterized in that: Made from the indium tin oxide material according to any one of claims 1 to 4.

10. The method for preparing the transparent conductive oxide thin film according to claim 9, characterized in that: The steps include: The indium tin oxide material according to any one of claims 1 to 4 is deposited on a substrate to obtain the transparent conductive oxide film.