A process for improving the grinding efficiency of high-grade nickel matte
Through the screening of ball mill and vibrating screen, and then the grading treatment of vertical mill and grader, the problem of different ore slurry particle size in high ice nickel grinding is solved, the particle size uniformity and resource utilization are achieved, and the grinding is improved and leaching efficiency reduces resource waste.
Patent Information
- Application Number
- CN202310230424.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-11
AI Technical Summary
Traditional grinding methods lead to different slurry particle sizes in high-ice nickel grinding, affecting leaching efficiency and causing waste of resources.
The process of ball mill + vibrating screen + vertical mill + classifier is adopted to treat high ice nickel samples through screening and grading to ensure the uniformity of particle size and achieve full utilization of resources.
It improves grinding and leaching efficiency, reduces resource waste, meets the particle size requirements of subsequent processes, and improves the utilization rate of raw materials.
Smart Images

Figure CN116078526B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of grinding, and in particular relates to a process for improving the grinding efficiency of high-grade nickel matte. Background Art
[0002] High-grade nickel matte is a sulfide eutectic of metals such as nickel, copper, cobalt, and iron formed by primary smelting of nickel concentrate in an electric converter. It is used to produce electrolytic nickel, nickel oxide, nickel-iron, nickel-containing alloys and various nickel salts. After special treatment, it can also be directly used for steelmaking. After grinding, high-grade nickel matte is leached with sulfuric acid solution to extract high-purity metallic nickel and nickel alloys. The traditional grinding method only uses a grinding machine to grind and crush the ore and then conduct subsequent leaching, which will produce larger metal alloy flakes. The particle size and particle size distribution of the ground slurry are different, which directly affects the grinding efficiency and subsequent leaching efficiency. Materials with too large particles cannot be reused, which will also cause waste of resources. Summary of the invention
[0003] The purpose of the present invention is to provide a process for improving the grinding efficiency of high-grade nickel matte, so as to solve the problem that the traditional grinding method affects the grinding and leaching efficiency and causes waste of resources.
[0004] The technical solution of the present invention is: a process for improving the grinding efficiency of high-grade nickel matte, characterized in that it comprises the following steps:
[0005] Step 1: Grind the high-grade nickel matte sample through a grinding device, sieve the slurry discharged from the grinding through a screener, and use the sieved material directly for metal leaching;
[0006] Step 2: placing the screened material in step 1 into a vertical mill for grinding, and then classifying it through a classifier. The overflow product is collected and used for leaching nickel liquid after slurrying and batching.
[0007] Step 3: Place the sediment obtained by classification in step 2 back into the vertical mill, and repeat the operation until the product of the required particle size does not overflow after classification, and then stop the operation.
[0008] Furthermore, the nickel content of the high nickel matte sample in step one is 65%, and the particle size is ≤3mm.
[0009] Furthermore, the particle size of the sieved material in step 2 is -190 mesh.
[0010] Furthermore, the particle size of the classified product in step 2 is -280 mesh.
[0011] Furthermore, the grinding equipment in step one is a ball mill.
[0012] Furthermore, in step one, the screener is a vibrating screen.
[0013] Furthermore, the classifier in step 2 is a spiral classifier or a cyclone.
[0014] The beneficial effects of the present invention are as follows: a grinding process of a first-stage ball mill + a vibrating screen + a second-stage vertical mill + a classifier is adopted, the process is simple and effective, the alloy phase screened out by the ball mill for the first grinding can be directly dissolved and leached with acid solution, the remaining product is ground again by the vertical mill and then classified, and the -280 mesh product obtained by classification can be leached into nickel liquid after slurry batching, which solves the problem that the particle size of the ore pulp ground by the traditional grinding method is different, affecting the grinding efficiency and leaching efficiency, and realizes that the particle size distribution of the grinding slurry is uniform and the particle size meets the requirements of the subsequent process, which is helpful to improve the leaching efficiency, and at the same time, the material raw materials can be used more fully without causing waste of resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0016] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.
[0017] Embodiment 1,
[0018] like Figure 1 As shown, a process for improving the grinding efficiency of high-grade nickel matte comprises the following steps:
[0019] Step 1: Grind the high nickel matte sample with a nickel content of 65% and a particle size of ≤3 mm through a ball mill, and screen the slurry discharged from the grinding through a vibrating screen with a -190 mesh screen. The sieve-surface material is the alloy phase, and the sieve-underface material is the -190 mesh product. The sieve-surface material is directly leached with an acidic solution for metal extraction;
[0020] Step 2: Place the -190 mesh product in step 1 into a vertical mill for grinding, and then classify it through a classifier, and collect the -280 mesh product overflowing from the classification;
[0021] The collected -280 mesh product can be used for leaching nickel solution after being slurried and mixed.
[0022] Step 3: Place the sediment obtained by classification in step 2 back into the vertical mill, and repeat the operation until the product of the required particle size does not overflow after classification, and then stop the operation.
[0023] Table 1 is a comparison between the grinding process of the present invention and the original treatment process in Example 1:
[0024]
[0025] Table 1
[0026] It can be seen from Table 1 that, under the condition of the same grinding processing capacity, by adopting the process flow of the present invention, the unit consumption of ball mill steel balls is reduced by 15%, the unit consumption of vertical mill steel balls is reduced by 16.7%, the power of ball mill is reduced by 10.2%, the power of vertical mill is reduced by 8.3%, the graded overflow -280 mesh product accounts for more than 90% of the raw materials, the concentration is ≥35%, the utilization rate of high nickel matte sample raw materials is maximized, and the product indicators meet the requirements of the use indicators, which effectively improves the utilization rate of raw materials and reduces resource waste.
Claims
1. A process for improving the grinding efficiency of high-grade nickel matte, characterized in that: The following steps are involved: Step 1: Grind the high-grade nickel matte sample through a grinding device, screen the slurry discharged from the grinding through a screener, and use the screened material directly for leaching metal. The high-grade nickel matte sample has a nickel content of 65% and a particle size of ≤3 mm; Step 2: placing the screened material in step 1 into a vertical mill for grinding, and then classifying it through a classifier. The particle size of the screened material is -190 mesh. The overflow product of the classification is collected and used for leaching nickel liquid after slurry batching. The particle size of the collected overflow product of the classification is -280 mesh. Step 3: Place the sediment obtained by classification in step 2 back into the vertical mill, and repeat the operation until the product of the required particle size does not overflow after classification, and then stop the operation.
2. A process for improving the grinding efficiency of high-grade nickel matte according to claim 1, characterized in that: The grinding equipment in step 1 is a ball mill.
3. A process for improving the grinding efficiency of high-grade nickel matte according to claim 1, characterized in that: In the step 1, the screener is a vibrating screen.
4. A process for improving the grinding efficiency of high-grade nickel matte according to claim 1, characterized in that: The classifier in step 2 is a spiral classifier or a cyclone.
Citation Information
Patent Citations
Non-cyanide ore dressing method for gold-copper-lead sulfide ore
CN102527498A
Method and equipment for extracting gold and silver from smelting slag
CN103882240A
Mineral separation and enrichment method for primary scandium ore
CN105435958A
Beneficiation process of copper-nickel sulfide ore
CN106622636A
Nickel recycling method
CN107630146A