Modified polylactic acid material, preparation method thereof and tableware

By adding an appropriate amount of iron into the polylactic acid material, the problem of the viscosity of polylactic acid material decreased in the aging test was solved, and its aging resistance was significantly improved, the high viscosity retention rate of polylactic acid material was achieved, and the material aging was delayed process.

CN116102858BActive Publication Date: 2024-11-26KINGFA SCI & TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310078358.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-26
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

The viscosity of polylactic acid materials dropped rapidly in simulated accelerated aging test, which affected their aging resistance and limited their large-scale promotion and application.

Method used

Iron is incorporated into polylactic acid materials, and by adjusting the mass proportion and source of iron, combined with specific polylactic acid resin preparation methods and molding processes, modifying polylactic acid materials are prepared to improve their viscosity maintenance in the aging test Rate.

Benefits of technology

The viscosity retention rate of modified polylactic acid materials reached more than 50% after simulated and accelerated aging test, which significantly improved its aging resistance and delayed the viscosity drop of polylactic acid materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004072042440000151
    Figure BDA0004072042440000151
  • Figure BDA0004072042440000152
    Figure BDA0004072042440000152
  • Figure BDA0004072042440000161
    Figure BDA0004072042440000161
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer materials, and in particular to a modified polylactic acid material and a preparation method thereof. The modified polylactic acid material comprises polylactic acid resin and iron element; the mass proportion of the iron element in the modified polylactic acid material is 3ppm to 700ppm. After an accelerated aging test, the modified polylactic acid material of the present invention has a good viscosity retention rate and has excellent aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to modified polylactic acid materials, a preparation method thereof, and tableware. Background Art

[0002] Corn rich in starch can be used through modern biotechnology to produce a colorless and transparent liquid - lactic acid, which can then be transformed into a granular polymer material - polylactic acid (PLA) material through a special polymerization process.

[0003] PLA material has the best tensile strength, but at this stage, the large-scale promotion and application of PLA material as a general plastic is still subject to certain restrictions. This is mainly due to the poor aging resistance of PLA material. For example, in simulated accelerated aging tests, the viscosity drops too quickly, affecting its use. Summary of the invention

[0004] Based on this, the present invention provides a modified polylactic acid material and a preparation method thereof and tableware to solve the problem that the PLA material has poor aging resistance.

[0005] The first aspect of the present invention provides a modified polylactic acid material. The technical solution is as follows:

[0006] A modified polylactic acid material, comprising polylactic acid resin and iron element;

[0007] Wherein, the mass proportion of iron element in the modified polylactic acid material is 3ppm to 700ppm.

[0008] In some of the embodiments, the mass proportion of iron in the modified polylactic acid material is 3ppm to 300ppm.

[0009] In some of the embodiments, the mass proportion of iron in the modified polylactic acid material is 5ppm to 80ppm.

[0010] In some embodiments, the iron element is derived from one or more of iron salts and iron oxides.

[0011] In some embodiments, the iron salt is selected from one or more of iron sulfate, iron nitrate and iron halide.

[0012] In some embodiments, the iron oxide is selected from one or more of ferrous oxide, ferrosinite and ferric oxide.

[0013] In some embodiments, the weight average molecular weight of the polylactic acid resin is 100,000 to 250,000.

[0014] In some of the embodiments, the terminal carboxyl content of the polylactic acid resin is 15 mol / t to 40 mol / t.

[0015] In some embodiments, the method for preparing the polylactic acid resin comprises the following steps:

[0016] mixing L-lactic acid and a first catalyst to carry out a polycondensation reaction to generate a lactide intermediate;

[0017] The lactide intermediate, an initiator and a second catalyst are mixed to carry out a ring-opening polymerization reaction to generate a polylactic acid resin.

[0018] In some embodiments, the first catalyst is stannous octoate.

[0019] In some embodiments, the second catalyst is stannous octoate.

[0020] In some embodiments, the initiator is ethylene glycol.

[0021] In some of the embodiments, the conditions of the polycondensation reaction include: reaction temperature of 80-140° C., reaction pressure of 3 KPa-8 KPa, and reaction time of 6 h-12 h.

[0022] In some embodiments, the ring-opening polymerization reaction includes at least two stages. The conditions of the first stage include: reaction temperature of 140-160°C, reaction pressure of 105000Pa-115000Pa, and reaction time of 3h-5h; the conditions of the second stage include: reaction temperature of 170-190°C, reaction pressure of 105000Pa-115000Pa, and reaction time of 2h-3h.

[0023] In some embodiments, after the modified polylactic acid material is placed at a temperature of 60° C. and a humidity of 60% for 9 days, the viscosity retention rate is not less than 50%.

[0024] The second aspect of the present invention provides a method for preparing a modified polylactic acid material. The technical scheme is as follows:

[0025] A method for preparing a modified polylactic acid material comprises the following steps:

[0026] Mixing polylactic acid resin and an iron-containing compound, and processing the obtained mixture into a shape to prepare a modified polylactic acid material;

[0027] The added amounts of the polylactic acid resin and the iron-containing compound satisfy the requirement that the mass proportion of the iron element in the modified polylactic acid material is 3ppm to 700ppm.

[0028] In some embodiments, the processing and molding method includes extrusion molding, injection molding, blown film molding, foaming molding or vacuum molding.

[0029] In some embodiments, the extrusion molding temperature is 140°C to 240°C.

[0030] A third aspect of the present invention provides tableware, which comprises the modified polylactic acid material or the modified polylactic acid material prepared by the above preparation method.

[0031] Compared with the traditional solution, the present invention has the following beneficial effects:

[0032] The inventor of the present invention unexpectedly discovered in the research that adding iron to the polylactic acid material is conducive to alleviating the viscosity drop of the polylactic acid material in the aging test, and the amount of iron is crucial to the presentation of the above effect. The reason may be that the addition of iron reduces the activity of the terminal carboxyl or terminal hydroxyl groups of the polylactic acid resin, controls the polylactic acid resin to be difficult to hydrolyze, and then delays the viscosity drop of the polylactic acid material. The modified polylactic acid material of the present invention has a higher viscosity retention rate (reaching more than 50%) after the simulated accelerated aging test, showing excellent aging resistance. DETAILED DESCRIPTION

[0033] The present invention will be further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0035] the term

[0036] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0037] In the present invention, "plurality", "multiple", "multiple times", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.

[0038] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of the present invention.

[0039] In the present invention, the words “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.

[0040] In the present invention, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0041] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0042] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0043] In the present invention, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.

[0044] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0045] In the present invention, when it comes to percentage content, unless otherwise specified, for solid-liquid mixing and solid-solid mixing, it refers to mass percentage, and for liquid-liquid mixing, it refers to volume percentage.

[0046] In the present invention, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.

[0047] The inventors of the present invention unexpectedly discovered during research that adding iron-containing compounds to polylactic acid materials is beneficial to alleviating the viscosity drop of polylactic acid materials in aging tests, and the content of iron elements is crucial to the presentation of the above-mentioned effect.

[0048] In one embodiment of the present invention, a modified polylactic acid material is provided, comprising polylactic acid resin and iron element;

[0049] The mass proportion of iron element in the modified polylactic acid material is 3ppm to 700ppm.

[0050] It can be understood that the mass proportion of iron element in the modified polylactic acid material includes but is not limited to 3ppm, 4ppm, 5ppm, 10ppm, 40ppm, 60ppm, 80ppm, 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 600ppm, and 700ppm.

[0051] In some preferred embodiments, the mass proportion of iron in the modified polylactic acid material is 3ppm to 300ppm.

[0052] In some further preferred embodiments, the mass proportion of iron element in the modified polylactic acid material is 5ppm to 80ppm.

[0053] Adding iron to the modified polylactic acid material can alleviate the viscosity decrease of the polylactic acid material in the aging test and improve its aging resistance. The reason may be that the addition of iron reduces the activity of the terminal carboxyl or terminal hydroxyl groups of the polylactic acid resin, controls the polylactic acid resin to be difficult to hydrolyze, and thus delays the viscosity decrease of the polylactic acid material.

[0054] Optionally, the iron element comes from one or more of iron salts and iron oxides.

[0055] Wherein, the iron salt is selected from one or more of iron sulfate, iron nitrate and iron halide. It can be understood that the iron salt can be a divalent iron salt or a trivalent iron salt. For example: ferrous sulfate, ferrous nitrate, ferrous chloride, ferric sulfate, ferric nitrate, ferric chloride, etc.

[0056] The iron oxide is selected from one or more of ferrous oxide, ferrosoferric oxide and ferric oxide.

[0057] The addition of the above-mentioned iron element can not only improve the aging resistance of the polylactic acid material, but also help to improve the tensile strength of the polylactic acid material.

[0058] In this embodiment, the weight average molecular weight of the polylactic acid resin is 80,000 to 200,000.

[0059] In this embodiment, the terminal carboxyl content of the polylactic acid resin is 15 mol / t to 40 mol / t.

[0060] Optionally, the preparation method of polylactic acid resin comprises the following steps:

[0061] mixing L-lactic acid and a first catalyst to carry out a polycondensation reaction to generate a lactide intermediate;

[0062] The lactide intermediate, an initiator and a second catalyst are mixed to carry out a ring-opening polymerization reaction to generate a polylactic acid resin.

[0063] Optionally, the first catalyst is stannous octoate.

[0064] Optionally, the second catalyst is stannous octoate.

[0065] Optionally, the initiator is ethylene glycol.

[0066] Optionally, the conditions of the polycondensation reaction include: reaction temperature of 80 to 140° C., reaction pressure of 3 KPa to 8 KPa, and reaction time of 6 h to 12 h.

[0067] It can be understood that after the polycondensation reaction, the oligomers generated by the polycondensation reaction are distilled under reduced pressure to obtain a lactide intermediate.

[0068] Optionally, the conditions for the reduced pressure distillation include: a temperature of 170 to 210° C. and a pressure of 102 Pa to 103 Pa. The reduced pressure distillation is performed until no product is distilled out, and the time may be 7 h to 15 h.

[0069] Optionally, the ring-opening polymerization reaction includes at least two stages, and the conditions of the first stage include: reaction temperature of 140-160°C, reaction pressure of 105000Pa-115000Pa, and reaction time of 3h-5h; the conditions of the second stage include: reaction temperature of 170-190°C, reaction pressure of 105000Pa-115000Pa, and reaction time of 2h-3h.

[0070] It can be understood that the ring-opening polymerization reaction is performed, and the polymer generated by the ring-opening polymerization reaction is dissolved in a chloroform aqueous solution and then precipitated with ethanol to obtain a polylactic acid resin.

[0071] In this embodiment, after the modified polylactic acid material is placed at a temperature of 60° C. and a humidity of 60% for 9 days, the viscosity retention rate is not less than 50%.

[0072] The present invention also provides a method for preparing a modified polylactic acid material. In one embodiment, the method for preparing a modified polylactic acid material comprises the following steps:

[0073] Mixing polylactic acid resin and an iron-containing compound, and processing the obtained mixture into a shape to prepare a modified polylactic acid material;

[0074] The added amounts of the polylactic acid resin and the iron-containing compound satisfy the requirement that the mass proportion of the iron element in the modified polylactic acid material is 3ppm to 700ppm.

[0075] It can be understood that the polylactic acid resin in the preparation method of the modified polylactic acid material is the same as the polylactic acid resin in the modified polylactic acid material, and no further description is given here.

[0076] Those skilled in the art know that when a small amount of an iron-containing compound is added to a large amount of polylactic acid resin, the two can be mixed evenly by pre-mixing for multiple times.

[0077] It is understandable that the iron-containing compound is selected from one or more of iron salts and iron oxides, wherein the iron salts and iron oxides are as described above and will not be described in detail herein.

[0078] Optionally, the processing and molding methods include extrusion molding, injection molding, film blowing molding, foaming molding or vacuum molding.

[0079] In this embodiment, the processing and molding method is extrusion molding, and the extrusion molding temperature is 140°C to 240°C.

[0080] In one embodiment of the present invention, tableware is provided, which comprises the modified polylactic acid material or the modified polylactic acid material prepared by the preparation method. The tableware includes but is not limited to disposable bowls, disposable cups, disposable plates, etc.

[0081] The following is further described in conjunction with specific examples and comparative examples. The raw materials involved in the following specific examples, unless otherwise specified, can all be sourced from commercial sources. The instruments used, unless otherwise specified, can all be sourced from commercial sources. The processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0082] Example 1

[0083] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0084] Step 1: Preparation of polylactic acid resin

[0085] (1) Add L-lactic acid and a first catalyst (stannous octoate) accounting for 0.04 wt% of the L-lactic acid into a reaction vessel, stir evenly, and carry out polycondensation reaction at a temperature of 100° C. and a pressure of 5 KPa. After 9 hours, distill off water to obtain an oligomer. The obtained oligomer is distilled under reduced pressure at a temperature of 190° C. and a pressure of 102 Pa until no product is distilled out. The time is 11 hours to obtain a lactide intermediate.

[0086] (2) The lactide intermediate obtained in the above step is dissolved in an initiator (hexanediol) accounting for 0.24 wt% of the lactide intermediate, and a second catalyst (stannous octoate) accounting for 0.04 wt% of the lactide intermediate is added to carry out a ring-opening polymerization reaction, specifically: first react at a temperature of 150° C. and a relative pressure of 110,000 Pa for 4 hours, and then react at a temperature of 180° C. and a relative pressure of 110,000 Pa for 2.5 hours to obtain a polymer, and the obtained polymer solid is refluxed and dissolved with a 5% (W / W) chloroform aqueous solution. After the solution is filtered, it is precipitated with ethanol 5 times the volume of chloroform to obtain a white flocculent precipitate to obtain a polylactic acid resin. The weight average molecular weight of the obtained polylactic acid resin is 200000, and the terminal carboxyl content is 40 mol / t, wherein the method for determining the terminal carboxyl content is: using a mixed solution of o-cresol and chloroform in a mass ratio of 7:3 as a solvent, using a Swiss Metrohm Titrino series automatic potentiometric titrator to test the terminal carboxyl value, and the test method implements FZ / T 50012-2006 "Determination of Terminal Carboxyl Content in Polyester-Titration Analysis Method".

[0087] Step 2: Preparation of modified polylactic acid material

[0088] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 was uniformly mixed with 0.43 g of ferric oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0089] The aging resistance of the modified polylactic acid material prepared in step 2 was evaluated. The evaluation method is as follows. The evaluation results are shown in Table 1.

[0090] Before and after the simulated accelerated aging test, the intrinsic viscosity of the modified polylactic acid material was measured respectively. According to the public: viscosity retention rate = (η 前 -η 后 ) / η 前 × 100%, calculate the viscosity retention rate.

[0091] Among them, the test method for the characteristic viscosity η of the modified polylactic acid material is as follows: at 23°C, accurately weigh 0.1250±0.0005g of the sample and dissolve it in 25mL (o-dichlorobenzene: phenol = 2:3 mass ratio) solution, heat and stir at 110°C until the modified polylactic acid material is completely dissolved, and measure it with a viscometer at 23°C, and retain two decimal places for the viscosity value.

[0092] The conditions of the simulated accelerated aging test are as follows: temperature of 60°C, humidity of 60%, and placement for 9 days.

[0093] Example 2

[0094] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0095] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 0.55 g of ferrosoferric oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0096] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0097] Example 3

[0098] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0099] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 0.64 g of ferrous oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0100] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0101] Example 4

[0102] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0103] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 2.99 g of ferrous sulfate, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0104] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0105] Example 5

[0106] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0107] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 12.5 g of ferric sulfate, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0108] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0109] Example 6

[0110] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0111] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 27 g of ferrous nitrate, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0112] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0113] Example 7

[0114] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0115] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 32 g of ferric nitrate, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0116] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0117] Example 8

[0118] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0119] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 15 g of ferrous oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0120] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0121] Example 9

[0122] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0123] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 40 g of ferrous oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0124] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0125] Example 10

[0126] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0127] Referring to Table 1, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 92 g of ferrous oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0128] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0129] Embodiment 11

[0130] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0131] Step 1: Preparation of polylactic acid resin

[0132] (1) Add L-lactic acid and a first catalyst (stannous octoate) accounting for 0.04 wt% of the L-lactic acid into a reaction vessel, stir evenly, and carry out polycondensation reaction at a temperature of 100° C. and a pressure of 5 KPa. After 9 hours, distill off water to obtain an oligomer. The obtained oligomer is distilled under reduced pressure at a temperature of 190° C. and a pressure of 102 Pa until no product is distilled out. The time is 11 hours to obtain a lactide intermediate.

[0133] (2) The lactide intermediate obtained in the above step is dissolved in an initiator (hexanediol) accounting for 0.4 wt% of the lactide intermediate, and a second catalyst (stannous octoate) accounting for 0.04 wt% of the lactide intermediate is added to carry out a ring-opening polymerization reaction, specifically: first react at a temperature of 150° C. and a relative pressure of 110,000 Pa for 4 hours, and then react at a temperature of 180° C. and a relative pressure of 110,000 Pa for 2.5 hours to obtain a polymer, and the obtained polymer solid is refluxed and dissolved with a 5% (W / W) chloroform aqueous solution, and after the solution is filtered, ethanol 5 times the volume of chloroform is used for precipitation to obtain a white flocculent precipitate to obtain a polylactic acid resin. The weight average molecular weight of the obtained polylactic acid resin is 80,000, and the terminal carboxyl content is 15 mol / t.

[0134] Step 2: Preparation of modified polylactic acid material

[0135] Referring to Table 2, 100 kg of the polylactic acid resin prepared in step 1 was evenly mixed with 0.43 g of ferric oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0136] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0137] Example 12

[0138] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0139] Step 1: Preparation of polylactic acid resin

[0140] (1) Add L-lactic acid and a first catalyst (stannous octoate) accounting for 0.04 wt% of the L-lactic acid into a reaction vessel, stir evenly, and carry out polycondensation reaction at a temperature of 100° C. and a pressure of 5 KPa. After 9 hours, distill off water to obtain an oligomer. The obtained oligomer is distilled under reduced pressure at a temperature of 190° C. and a pressure of 102 Pa until no product is distilled out. The time is 11 hours to obtain a lactide intermediate.

[0141] (2) The lactide intermediate obtained in the above step is dissolved in an initiator (hexanediol) accounting for 0.45 wt% of the lactide intermediate, and a second catalyst (stannous octoate) accounting for 0.04 wt% of the lactide intermediate is added to carry out a ring-opening polymerization reaction, specifically: first react at a temperature of 150° C. and a relative pressure of 110,000 Pa for 4 hours, and then react at a temperature of 180° C. and a relative pressure of 110,000 Pa for 2.5 hours to obtain a polymer, and the obtained polymer solid is refluxed and dissolved with a 5% (W / W) chloroform aqueous solution, and after the solution is filtered, ethanol 5 times the volume of chloroform is used for precipitation to obtain a white flocculent precipitate to obtain a polylactic acid resin. The weight average molecular weight of the obtained polylactic acid resin is 50,000, and the terminal carboxyl content is 10 mol / t.

[0142] Step 2: Preparation of modified polylactic acid material

[0143] Referring to Table 2, 100 kg of the polylactic acid resin prepared in step 1 was evenly mixed with 0.43 g of ferric oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0144] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0145] Embodiment 13

[0146] This embodiment provides a modified polylactic acid material and a preparation method thereof, the steps are as follows:

[0147] Step 1: Preparation of polylactic acid resin

[0148] (1) Add L-lactic acid and a first catalyst (stannous octoate) accounting for 0.04 wt% of the L-lactic acid into a reaction vessel, stir evenly, and carry out polycondensation reaction at a temperature of 100° C. and a pressure of 5 KPa. After 9 hours, distill off water to obtain an oligomer. The obtained oligomer is distilled under reduced pressure at a temperature of 190° C. and a pressure of 102 Pa until no product is distilled out. The time is 11 hours to obtain a lactide intermediate.

[0149] (2) The lactide intermediate obtained in the above step is dissolved in an initiator (hexanediol) accounting for 0.2 wt% of the lactide intermediate, and a second catalyst (stannous octoate) accounting for 0.04 wt% of the lactide intermediate is added to carry out a ring-opening polymerization reaction, specifically: first react at a temperature of 150° C. and a relative pressure of 110,000 Pa for 4 hours, and then react at a temperature of 180° C. and a relative pressure of 110,000 Pa for 2.5 hours to obtain a polymer, and the obtained polymer solid is refluxed and dissolved with a 5% (W / W) chloroform aqueous solution, and after the solution is filtered, ethanol 5 times the volume of chloroform is used for precipitation to obtain a white flocculent precipitate to obtain a polylactic acid resin. The weight average molecular weight of the obtained polylactic acid resin is 300,000, and the terminal carboxyl content is 20 mol / t.

[0150] Step 2: Preparation of modified polylactic acid material

[0151] Referring to Table 2, 100 kg of the polylactic acid resin prepared in step 1 was evenly mixed with 0.43 g of ferric oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a modified polylactic acid material.

[0152] The aging resistance of the prepared modified polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0153] Table 1

[0154]

[0155] Table 2

[0156]

[0157]

[0158] Among them, the test of the mass proportion of Fe element is tested by microwave digestion-ICP-OES method, and the unit of measurement result is ppm, where 1ppm=0.001‰. Specifically: weigh 0.1g of the crushed modified polylactic acid material as a sample, put it into a microwave digestion tank, add 5mL of nitric acid to completely immerse the sample, and then slowly drip 1.0mL of hydrogen peroxide. After reacting for 2 minutes, cover the lid, seal the digestion tank, put it into a microwave digestion furnace for digestion, cool to room temperature, filter the solution in the digestion tank with a 0.45μm filter membrane, transfer it to a volumetric flask, dilute it to 50mL with distilled water, and use ICP-OES test.

[0159] As shown in Table 1, in Example 1-Example 13, iron element is added to the modified polylactic acid material by adding iron-containing compounds. After testing, the amount of Fe added is 3ppm~700ppm. After adding iron element, the modified polylactic acid material has a higher viscosity retention rate (all reaching more than 50%) after the simulated accelerated aging test, showing excellent aging resistance. With the change of the mass of iron element, the viscosity retention rate of the modified polylactic acid material also changes. With the change of the weight average molecular weight and terminal hydroxyl content of the polylactic acid resin, the viscosity retention rate of the aging-resistant polylactic acid material also changes. Among them, after testing, when the amount of Fe added is 5ppm~80ppm, the aging-resistant polylactic acid material has a viscosity retention rate of more than 75% after the simulated accelerated aging test, and the effect is better. When the weight average molecular weight of the polylactic acid resin is 80000~200000 and the terminal carboxyl content is 5~40mol / t, the aging-resistant polylactic acid material has a viscosity retention rate of more than 64% after the simulated accelerated aging test, and the effect is better.

[0160] Comparative Example 1

[0161] This comparative example provides a polylactic acid material and a preparation method thereof, the steps are as follows:

[0162] Referring to Table 3, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was put into a single screw extruder, extruded and granulated at 190° C. to obtain a polylactic acid material.

[0163] The aging resistance of the prepared polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0164] Comparative Example 2

[0165] This comparative example provides a polylactic acid material and a preparation method thereof, the steps are as follows:

[0166] Referring to Table 3, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 136 g of ferrous oxide, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a polylactic acid material.

[0167] The aging resistance of the prepared polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0168] Comparative Example 3

[0169] This comparative example provides a polylactic acid material and a preparation method thereof, the steps are as follows:

[0170] Referring to Table 3, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 1.56 g of zinc sulfate, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a polylactic acid material.

[0171] The aging resistance of the prepared polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0172] Comparative Example 4

[0173] This comparative example provides a polylactic acid material and a preparation method thereof, the steps are as follows:

[0174] Referring to Table 3, 100 kg of the polylactic acid resin prepared in step 1 of Example 1 was uniformly mixed with 8.5 g of cupric chloride, and the resulting mixture was put into a single-screw extruder, extruded and granulated at 190° C. to obtain a polylactic acid material.

[0175] The aging resistance of the prepared polylactic acid material was evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0176] Table 3

[0177]

[0178] Among them, the test of the mass proportion of metal elements is tested by microwave digestion-ICP-OES method, and the unit of measurement result is ppm, where 1ppm=0.001‰. Specifically: weigh 0.1g of crushed polylactic acid material or modified polylactic acid material as a sample, put it into a microwave digestion tank, add 5mL of nitric acid to completely immerse the sample, and then slowly drip 1.0mL of hydrogen peroxide. After reacting for 2 minutes, cover the lid, seal the digestion tank, and put it into a microwave digestion furnace for digestion. After cooling to room temperature, filter the solution in the digestion tank with a 0.45μm filter membrane and transfer it to a volumetric flask, dilute it to 50mL with distilled water, and use ICP-OES test.

[0179] As shown in Table 3, in Comparative Example 1, no iron-containing compound was added, and the polylactic acid material directly prepared from polylactic acid resin as raw material had a low viscosity retention rate (47%) after the simulated accelerated aging test, and had poor aging resistance.

[0180] In Comparative Example 2, although an iron-containing compound is added, the aging resistance of the modified polylactic acid material cannot be effectively improved due to the inappropriate amount of iron-containing compound added (in Comparative Example 2, the amount of iron element added is 1050 ppm, and the viscosity retention rate is 50%). Combined with Examples 1 to 13, the mass proportion of iron element is controlled within a certain range (3ppm to 700ppm), which can maintain the viscosity retention rate of the polylactic acid material at 52% to 80%, and can have an unexpected effect on improving the aging resistance of the modified polylactic acid material.

[0181] In Comparative Example 3, the aging resistance of the modified polylactic acid material prepared by adding the zinc-containing compound was not significantly improved, and even the viscosity retention rate decreased (the viscosity retention rate was 48%).

[0182] In Comparative Example 4, the modified polylactic acid material prepared by adding the copper-containing compound showed a significant decrease in viscosity retention, and the aging resistance decreased instead of increased (viscosity retention was 35%).

[0183] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0184] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A modified polylactic acid material, characterized in that: Includes polylactic acid resin and iron element; Wherein, the mass proportion of iron element in the modified polylactic acid material is 3ppm to 700ppm; The iron element is derived from one or more of iron salts and iron oxides; The iron salt is selected from one or more of iron sulfate, iron nitrate and iron halide.

2. The modified polylactic acid material according to claim 1, characterized in that: The mass proportion of iron element in the modified polylactic acid material is 3ppm to 300ppm.

3. The modified polylactic acid material according to claim 2, characterized in that: The mass proportion of iron element in the modified polylactic acid material is 5ppm to 80ppm.

4. The modified polylactic acid material according to claim 1, characterized in that: The iron oxide is selected from one or more of ferrous oxide, ferrosoferric oxide and ferric oxide.

5. The modified polylactic acid material according to any one of claims 1 to 4, characterized in that: The weight average molecular weight of the polylactic acid resin is 80,000 to 200,000.

6. The modified polylactic acid material according to claim 5, characterized in that: The terminal carboxyl content of the polylactic acid resin is 15 mol / t to 40 mol / t.

7. The modified polylactic acid material according to claim 6, characterized in that: The preparation method of the polylactic acid resin comprises the following steps: mixing L-lactic acid and a first catalyst to carry out a polycondensation reaction to generate a lactide intermediate; The lactide intermediate, an initiator and a second catalyst are mixed to carry out a ring-opening polymerization reaction to generate the polylactic acid resin.

8. The modified polylactic acid material according to claim 7, characterized in that: The first catalyst is stannous octoate.

9. The modified polylactic acid material according to claim 7, characterized in that: The second catalyst is stannous octoate.

10. The modified polylactic acid material according to claim 7, characterized in that: The initiator is ethylene glycol.

11. The modified polylactic acid material according to claim 7, characterized in that: The conditions of the polycondensation reaction include: reaction temperature of 80-140° C., reaction pressure of 3 kPa-8 kPa, and reaction time of 6 h-12 h.

12. The modified polylactic acid material according to claim 7, characterized in that: The ring-opening polymerization reaction includes at least two stages. The conditions of the first stage include: reaction temperature of 140-160°C, reaction pressure of 105000Pa-115000Pa, and reaction time of 3h-5h; the conditions of the second stage include: reaction temperature of 170-190°C, reaction pressure of 105000Pa-115000Pa, and reaction time of 2h-3h.

13. The modified polylactic acid material according to any one of claims 1-4 and 6-12, characterized in that: The modified polylactic acid material meets the following characteristics: After being placed at a temperature of 60°C and a humidity of 60% for 9 days, the viscosity retention rate is not less than 50%.

14. A method for preparing a modified polylactic acid material, characterized in that: The following steps are involved: Mixing polylactic acid resin and an iron-containing compound, and processing the obtained mixture into a shape to prepare a modified polylactic acid material; The iron-containing compound is selected from one or more of iron salts and iron oxides; the iron salt is selected from one or more of iron sulfates, iron nitrates and iron halides; The added amounts of the polylactic acid resin and the iron-containing compound satisfy the requirement that the mass proportion of the iron element in the modified polylactic acid material is 3ppm to 700ppm.

15. A tableware, characterized in that: It includes the modified polylactic acid material according to any one of claims 1 to 13 or the modified polylactic acid material prepared by the preparation method according to claim 14.