Heat-resistant and wear-resistant coating of die steel for steering knuckle and preparation method thereof

By using Cr3C2-NiCr and Cr2O3-Nano-TiO2 composite coating on the surface of 5CrNiMo mold steel, a gradient coating was formed using plasma spraying technology, which solved the problem of insufficient thermal fatigue and wear resistance of mold steel in high-temperature environments, significantly improving It has heat and wear resistance and service life.

CN116103598BActive Publication Date: 2024-11-08SINO TRUK JINAN POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211270940.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-17
Publication Date
2024-11-08
Estimated Expiration
2042-10-17

AI Technical Summary

Technical Problem

5CrNiMo mold steel is prone to thermal fatigue cracks in high temperature environments, has a short service life and insufficient wear resistance, resulting in serious surface cracking and cavity wear, affecting its application range and production efficiency.

Method used

The composite spray coating of Cr3C2 and NiCr and the composite spray coating of Cr2O3 and Nano-TiO2 are used to form a gradient coating on the surface of the mold steel through plasma spraying technology to improve its heat and wear resistance.

Benefits of technology

It significantly improves the heat and wear resistance of mold steel, reduces friction and wear speed, extends service life, and improves thermal fatigue resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116103598B_ABST
    Figure CN116103598B_ABST
Patent Text Reader

Abstract

The invention discloses a heat-resistant and wear-resistant coating for a mold steel for a steering knuckle and a preparation method thereof. The heat-resistant and wear-resistant coating is composed of a 5CrNiMo mold steel substrate and is sequentially a first spray coating and a second spray coating outwardly. The first coating is a composite spray coating of Cr3C2 and NiCr, and the second coating is a composite spray coating of Cr2O3 and Nano‑TiO2. The preparation method comprises the following steps: coating component ratio, mold steel surface sandblasting, first spray coating mixing, first spray coating feeding, first spray coating spraying treatment, second spray coating mixing, second spray coating feeding, and second spray coating spraying treatment. The heat-resistant and wear-resistant coating of the invention has a gradient change in composition from the surface layer to the inside, is self-lubricating during wear, has good fatigue resistance, can significantly improve the heat resistance of the mold material, and realizes the performance requirements of hot working mold steel materials in industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a die steel coating and a preparation method thereof, in particular to a novel heat-resistant and wear-resistant coating of a die steel for a steering knuckle and a preparation method thereof, belonging to the technical field of metal surface treatment engineering. Background Art

[0002] With the rapid development of my country's automobile industry, the demand for a full range of commercial vehicles such as heavy trucks, medium trucks, and light trucks has increased rapidly, which has increased the demand for molds and the performance requirements for hot working molds have become higher and higher. The performance and life of molds directly affect the quality, processing cost and efficiency of automotive parts. At the same time, with the increasingly fierce competition in economic globalization, reducing the cost of mold maintenance and use is imminent for the development of industries such as automobiles.

[0003] 5CrNiMo steel has the advantages of good impact toughness, good hardenability and low manufacturing cost. It is widely used in the manufacture of various large and medium-sized forging hammer dies and trimming dies. Since this die steel will be subjected to huge impact loads in the working environment, it will cause uneven thermal stress and thermal strain during repeated heating and cooling, and it will also be subjected to friction between the flowing hot metal and the cavity surface. Therefore, its service life is short, and failure phenomena such as cracking, collapse, wear, and thermal fatigue often occur. In addition, this type of hot working die steel has a high carbon content and a low alloy content, poor high-temperature thermal stability, and poor thermal fatigue performance. When the operating temperature exceeds 600°C, the thermal hardness of the die steel decreases, and thermal fatigue cracks are prone to occur, which seriously affects its application range and service life. Therefore, under the premise of ensuring the good impact toughness of this series of hot working die steel, improving the thermal strength of the material and improving its heat resistance can significantly improve production efficiency and reduce production costs. Summary of the invention

[0004] The purpose of the present invention is to provide a new type of heat-resistant and wear-resistant coating for mold steel for steering knuckle and a preparation method thereof. By adopting coating composition design, plasma spraying and other processes, the coating composition gradient and excellent heat-resistant and wear-resistant coating preparation are achieved, which effectively improves the surface cracking and cavity wear phenomena caused by insufficient material toughness of the mold steel and low wear resistance of the forging model cavity surface, and improves its heat resistance and wear resistance.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A heat-resistant and wear-resistant coating for a mold steel for a steering knuckle and a preparation method thereof, wherein the heat-resistant and wear-resistant coating is composed of a 5CrNiMo mold steel substrate and a first spray coating and a second spray coating in sequence outward, wherein the first coating is Cr 3 C 2 Composite spray coating with NiCr, the second coating is Cr 2 O 3 With Nano-TiO 2The composite spray coating; the preparation method steps are as follows:

[0007] (1) Coating composition ratio: Cr 3 C 2 、NiCr、Cr 2 O 3 , Nano-TiO 2 The granules are used as raw materials, and the components are weighed according to the proportion;

[0008] (2) Sandblasting treatment of mold steel surface: The surface of 5CrNiMo hot working mold steel is cleaned and polished, and then sandblasted to prepare for the next spraying process;

[0009] (3) First spray coating mixture: weigh Cr 3 C 2 The NiCr powder was put into anhydrous ethanol and stirred evenly. After ultrasonic oscillation treatment for 5 to 10 minutes, it was kept at 60-80℃ in a vacuum furnace for 1-2 hours to obtain a uniformly mixed Cr 3 C 2 -NiCr powder particles;

[0010] (4) First spray layer feeding: Mix the Cr 3 C 2 -NiCr powder particles are added to the plasma spraying equipment and prepared for spraying process;

[0011] (5) Spraying treatment of the first spray layer: The first spray layer, namely CrNiMo, is sprayed on the surface of 5CrNiMo hot working die steel using plasma spraying technology. 3 C 2 -NiCr composite coating; spraying current is 515A, spraying voltage is 55V, argon flow rate is 40L / min, hydrogen flow rate is 3-6L / min, powder feeding rate is 40g / min, spraying distance is 120-150m, spray gun translation speed is 200mm / s, and spraying is repeated 4 times;

[0012] (6) Second spray coating mixture: weigh Cr 2 O 3 With Nano-TiO 2 The powder was put into anhydrous ethanol and stirred evenly. After ultrasonic oscillation treatment for 5 to 10 minutes, it was kept at 60-80℃ in a vacuum furnace for 1-2 hours to obtain a uniformly mixed Cr 2 O 3 and Nano-TiO 2 Powder particles;

[0013] (7) Second spray layer feeding: Mix the Cr 2 O 3 and Nano-TiO2 Powder particles are added to the plasma spray equipment and are ready for spraying process;

[0014] (8) Spraying treatment of the second spray layer: Plasma spraying technology is used to spray the first spray layer Cr of 5CrNiMo hot working die steel. 3 C 2 The surface of the NiCr coating is further sprayed with a second spray layer, namely Cr 2 O 3 With Nano-TiO 2 The process parameters of the spraying treatment are the same as those in step (5).

[0015] The Cr 3 C 2 、NiCr、Cr 2 O 3 and Nano-TiO 2 The particle size is 40 to 60 μm.

[0016] The Cr 3 C 2 、NiCr、Cr 2 O 3 , Nano-TiO 2 The particle purity is not less than 99.9%.

[0017] The Cr in the first sprayed layer 3 C 2 The mass fraction ratio of NiCr is 4:1.

[0018] The Cr in the second sprayed layer 2 O 3 With Nano-TiO 2 The mass fraction ratio is 2 to 4:1, preferably 4:1.

[0019] The sandblasting process is: suction sandblasting, 70-80 mesh brown corundum sand, sandblasting angle 60°, relative movement speed of spray gun / workpiece 40m / min, air pressure 0.5MPa, sandblasting distance 300mm.

[0020] The thickness of the first sprayed layer and the second sprayed layer are both 150-200 μm.

[0021] Beneficial effects of the present invention:

[0022] (1) The present invention adopts Cr with high hardness, wear resistance, heat resistance and structural stability. 3 C 2 , NiCr composite components to achieve high wear resistance of the coating; by controlling the plasma spraying parameters to make Cr 3 C 2-NiCr particles only partially melt on the surface, while 5CrNiMo alloy melts completely, achieving the preparation of wear-resistant coating with good interlayer bonding and dense structure.

[0023] (2) The present invention adopts Cr with high hardness, wear resistance, heat resistance and structural stability. 2 O 3 Cr with good chemical stability and lubricity 2 O 3 -Nano-TiO 2 The composite coating realizes the self-lubricating and heat-resistant function of the coating, and realizes the heat resistance under actual working conditions in the material service project to reduce the wear failure rate and increase the service life.

[0024] (3) The present invention is in Cr 3 C 2 -NiCr / 5CrNiMo hot working die steel for further preparation of Cr 2 O 3 With Nano-TiO 2 The coating with composite components realizes the dual functionality of wear resistance and heat resistance, and the composition gradient change of the coating can be achieved by controlling the process parameters.

[0025] The coating obtained by the method of the present invention has a gradient composition change from the surface to the inside, is self-lubricating during wear, has good fatigue resistance, can significantly improve the heat resistance of the mold material, and achieves the performance requirements for hot working mold steel materials in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a structural schematic diagram of the present invention;

[0027] Figure 2 This is the microstructure diagram of Example 1 of the present invention (800 times). DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The described embodiments are only a part of the present invention, rather than all embodiments. The following description of the embodiments is merely illustrative and does not serve as any limitation to the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] Preparation of heat-resistant and wear-resistant coating A for die steel for steering knuckle (such as Figure 1 The preparation method thereof is as follows:

[0031] (1) Coating composition ratio: Cr 3 C 2 、NiCr、Cr 2 O 3 , Nano-TiO 2 The granules are used as raw materials, and the content of each component is weighed according to the established ingredients;

[0032] (2) Substrate treatment: The hot working die steel is cut into blocks of a predetermined size, and then double-cleaned with acetone and alcohol to remove oil stains. After cleaning and drying, it is polished layer by layer with 200, 400, 600, 800, and 1000 mesh sandpaper, and then sandblasted. The suction sandblasting method is adopted, and brown corundum sand of about 75 mesh is selected. The sandblasting angle is 60°, the relative moving speed of the spray gun / workpiece is 40 m / min, the air pressure is 0.5 MPa, and the sandblasting distance is 300 mm, in preparation for the next spraying process;

[0033] (3) Mixing: weigh Cr 3 C 2 The mixture was put into anhydrous ethanol with NiCr powder in a ratio of 4:1 and stirred evenly. After being treated with ultrasonic oscillation for 5 minutes, the mixture was kept at 60°C in a vacuum furnace for 2 hours to obtain evenly mixed powder particles.

[0034] (4) Adding materials: Add the mixed Cr 3 C 2 -NiCr powder is added to the plasma spraying equipment and prepared for spraying process;

[0035] (5) Plasma spraying treatment of the first spray layer: Plasma spraying technology is used to spray Cr on the surface of 5CrNiMo hot working die steel. 3 C 2 -NiCr coating, spraying current is 515A, spraying voltage is 55V, argon flow rate is 40L / min, hydrogen flow rate is 3-6L / min, powder feeding rate is 40g / min, spraying distance: 120-150m, spray gun translation rate is 200mm / s, repeat spraying 4 times, and you can get a high wear-resistant coating (first spray layer) with excellent interlayer bonding and dense structure.

[0036] (6) Mixing: weigh the Cr 2 O 3 With Nano-TiO 2 The powder was put into anhydrous ethanol at a ratio of 4:1 and stirred evenly. After being treated with ultrasonic oscillation for 7 minutes, it was kept at 70°C in a vacuum furnace for 1.5 hours to obtain uniformly mixed powder particles. Finally, the coating powder after homogenization and mixing was added to the plasma spraying equipment to prepare for spraying processing.

[0037] (7) Plasma spraying treatment of the second spray layer: Plasma spraying technology is used to coat 5CrNiMo hot working die steel Cr 3 C 2 -NiCr coating surface is further sprayed with Cr 2 O 3 With Nano-TiO 2 Composite coating, spraying current is 515A, spraying voltage is 55V, argon flow rate is 40L / min, hydrogen flow rate is 3-6L / min, powder feeding rate is 40g / min, spraying distance: 120-150m, spray gun translation speed is 200mm / s, repeat spraying 4 times, you can get a self-lubricating gradient wear-resistant component coating (second spray layer).

[0038] According to GB / T8642-2002 "Determination of tensile bonding strength of thermal spraying", the bonding strength of the gradient heat-resistant and wear-resistant coating obtained in the above embodiment 1 is 39.5MPa, and the friction and wear performance of the coating is further tested. The high-temperature friction coefficient of the coating is tested by HT-1000 high-temperature friction and wear tester, with a load of 1N, a friction radius of 5mm, a rotation speed of 220r / min, a test time of 30min, a friction factor of 0.4, and an average wear scar width of 365.5μm. The test results show that the coating bonding strength of the steering knuckle mold steel of the present invention is excellent. During the friction and wear process, due to the heat resistance of its surface coating, the friction and wear speed of the material is reduced, the wear resistance of the material is improved, and the service life of the material is increased. In addition, after the sample of this embodiment has undergone an average of 120 and 50 thermal shock cycles at 400℃ and 550℃, respectively, the surface coating has not peeled off, and the main part of the cylinder is intact, indicating that the composite coating has good thermal fatigue resistance.

[0039] The 800 times microstructure of this embodiment is as follows Figure 1 shown.

[0040] Example 2

[0041] Preparation of heat-resistant and wear-resistant coating B for die steel for steering knuckle (such as Figure 1 The preparation method thereof is as follows:

[0042] (1) Coating composition ratio: Cr 3 C 2 、NiCr、Cr 2 O 3 , Nano-TiO 2 The granules are used as raw materials, and the content of each component is weighed according to the established ingredients;

[0043] (2) Substrate treatment: The hot working die steel is cut into blocks of a predetermined size, and then double-cleaned with acetone and alcohol to remove oil stains. After cleaning and drying, it is polished layer by layer with 200, 400, 600, 800, and 1000 mesh sandpaper, and then sandblasted. The suction sandblasting method is adopted, and brown corundum sand of about 75 mesh is selected. The angle is 60°, the relative moving speed of the spray gun / workpiece is 40 m / min, the air pressure is 0.5 MPa, and the sandblasting distance is 300 mm, in preparation for the next spraying process;

[0044] (3) Mixing: weigh Cr 3 C 2 The mixture was put into anhydrous ethanol with NiCr powder in a ratio of 4:1 and stirred evenly. After being treated with ultrasonic oscillation for 8 minutes, the mixture was kept at 80°C in a vacuum furnace for 1.5 hours to obtain evenly mixed powder particles.

[0045] (4) Adding materials: Add the mixed Cr 3 C 2 -NiCr powder is added to the plasma spraying equipment and prepared for spraying process;

[0046] (5) Plasma spraying treatment of the first spray layer: Plasma spraying technology is used to spray Cr on the surface of 5CrNiMo hot working die steel. 3 C 2 -NiCr coating, spraying current is 515A, spraying voltage is 55V, argon flow rate is 40L / min, hydrogen flow rate is 3-6L / min, powder feeding rate is 40g / min, spraying distance: 120-150m, spray gun translation rate is 200mm / s, repeat spraying 4 times, and you can get a high wear-resistant coating (first spray layer) with excellent interlayer bonding and dense structure.

[0047] (6) Mixing: weigh the Cr 2 O 3 With Nano-TiO 2 The powder was put into anhydrous ethanol at a ratio of 3:1 and stirred evenly. After being treated with ultrasonic oscillation for 10 minutes, it was kept at 75°C in a vacuum furnace for 2 hours to obtain uniformly mixed powder particles. Finally, the coating powder after homogenization and mixing was added to the plasma spraying equipment to prepare for spraying processing.

[0048] (7) Plasma spraying treatment of the second spray layer: Plasma spraying technology is used to coat 5CrNiMo hot working die steel Cr 3 C 2 -NiCr coating surface is further sprayed with Cr 2 O 3 With Nano-TiO 2Composite coating, spraying current is 515A, spraying voltage is 55V, argon flow rate is 40L / min, hydrogen flow rate is 3-6L / min, powder feeding rate is 40g / min, spraying distance: 120-150m, spray gun translation speed is 200mm / s, repeat spraying 4 times, you can get a self-lubricating gradient wear-resistant component coating (second spray layer).

[0049] According to GB / T8642-2002 "Determination of tensile bonding strength of thermal spraying", the bonding strength of the gradient heat-resistant and wear-resistant coating obtained in the above embodiment 2 is about 37.9MPa, and the friction and wear performance of the coating is further tested. The high-temperature friction coefficient of the coating is tested by HT-1000 high-temperature friction and wear tester, with a load of 1N, a friction radius of 5mm, a rotation speed of 220r / min, a test time of 30min, a friction factor of 0.43, and an average wear scar width of 371.3μm. The test results show that the coating bonding strength of the steering knuckle mold steel of the present invention is excellent. During the friction and wear process, due to the heat resistance of its surface coating, the friction and wear speed of the material is reduced, the wear resistance of the material is improved, and the service life of the material is increased. In addition, after the sample of this embodiment has undergone an average of 120 and 50 thermal shock cycles at 400℃ and 550℃, the surface coating has basically not peeled off, and the main part of the cylinder is intact, indicating that the composite coating has good thermal fatigue resistance.

[0050] Example 3

[0051] Preparation of heat-resistant and wear-resistant coating C of mold steel for steering knuckle, the preparation method and steps are as follows:

[0052] (1) Coating composition ratio: Cr 3 C 2 、NiCr、Cr 2 O 3 , Nano-TiO 2 The granules are used as raw materials, and the content of each component is weighed according to the established ingredients;

[0053] (2) Substrate treatment: The hot working die steel is cut into blocks of a predetermined size, and then double-cleaned with acetone and alcohol to remove oil stains. After cleaning and drying, it is polished layer by layer with 200, 400, 600, 800, and 1000 mesh sandpaper, and then sandblasted. The suction sandblasting method is adopted, and brown corundum sand of about 75 mesh is selected. The angle is 60°, the relative moving speed of the spray gun / workpiece is 40 m / min, the air pressure is 0.5 MPa, and the sandblasting distance is 300 mm, in preparation for the next spraying process;

[0054] (3) Mixing: weigh Cr 3 C 2The mixture was put into anhydrous ethanol at a ratio of 4:1 with NiCr powder and stirred evenly. After being treated with ultrasonic oscillation for 10 minutes, the mixture was kept at 80°C in a vacuum furnace for 1.5 hours to obtain evenly mixed powder particles.

[0055] (4) Adding materials: Add the mixed Cr 3 C 2 -NiCr powder is added to the plasma spraying equipment and prepared for spraying process;

[0056] (5) Plasma spraying treatment of the first spray layer: Plasma spraying technology is used to spray Cr on the surface of 5CrNiMo hot working die steel. 3 C 2 -NiCr coating, spraying current is 515A, spraying voltage is 55V, argon flow rate is 40L / min, hydrogen flow rate is 3-6L / min, powder feeding rate is 40g / min, spraying distance: 120-150m, spray gun translation rate is 200mm / s, repeat spraying 4 times, and you can get a high wear-resistant coating (first spray layer) with excellent interlayer bonding and dense structure.

[0057] (6) Mixing: weigh the Cr 2 O 3 With Nano-TiO 2 The powder was put into anhydrous ethanol at a ratio of 2:1 and stirred evenly. After being treated with ultrasonic oscillation for 8 minutes, it was kept at 60°C in a vacuum furnace for 1.5 hours to obtain uniformly mixed powder particles. Finally, the coating powder after homogenization and mixing was added to the plasma spraying equipment to prepare for spraying processing.

[0058] (7) Plasma spraying treatment of the second spray layer: Plasma spraying technology is used to coat 5CrNiMo hot working die steel Cr 3 C 2 -NiCr coating surface is further sprayed with Cr 2 O 3 With Nano-TiO 2 Composite coating, spraying current is 515A, spraying voltage is 55V, argon flow rate is 40L / min, hydrogen flow rate is 3-6L / min, powder feeding rate is 40g / min, spraying distance: 120-150m, spray gun translation speed is 200mm / s, repeat spraying 4 times, you can get a self-lubricating gradient wear-resistant component coating (second spray layer).

[0059] According to GB / T8642-2002 "Determination of tensile bonding strength of thermal spraying", the bonding strength of the gradient heat-resistant and wear-resistant coating obtained in the above embodiment 3 is about 35.2MPa, and the friction and wear performance of the coating is further tested. The high-temperature friction coefficient of the coating is tested by HT-1000 high-temperature friction and wear tester, with a load of 1N, a friction radius of 5mm, a rotation speed of 220r / min, a test time of 30min, a friction factor of 0.49, and an average wear scar width of 377.1μm. The test results show that the coating bonding strength of the steering knuckle mold steel of the present invention is excellent. During the friction and wear process, due to the heat resistance of its surface coating, the friction and wear speed of the material is reduced, the wear resistance of the material is improved, and the service life of the material is increased. After the sample has undergone an average of 120 and 50 thermal shock cycles at 400℃ and 550℃, respectively, there is basically no peeling, and the main part of the cylinder is intact, indicating that the composite coating has good thermal fatigue resistance.

[0060] Through the analysis of the bonding strength, friction and wear performance and thermal shock test results of the above embodiments, it can be seen that compared with the three coating structures of A, B and C, the coating structure A prepared in Example 1 is denser and has better strength, wear resistance and thermal fatigue resistance.

[0061] The present invention adopts plasma spraying technology to prepare Cr 3 C 2 -NiCr / 5CrNiMo hot working die steel material coating, using mold cavity processing three-dimensional solid scanning path for spraying to ensure stable spraying quality; control plasma spraying parameters to make Cr 3 C 2 -NiCr particles only partially melt on the surface, ensuring good interlayer bonding between the coating and the matrix components and compact organization. 3 C 2 -NiCr / 5CrNiMo wear-resistant coating is further prepared by using Cr 2 O 3 and Nano-TiO 2 The composite coating achieves wear resistance while satisfying the self-lubricating characteristics and composition gradient variability.

[0062] The above embodiments of the present invention are merely illustrative and not exclusive, and all modifications within the scope of the present invention or equivalent to the scope of the present invention are encompassed by the present invention.

Claims

1. A heat-resistant and wear-resistant coating for a mold steel for a steering knuckle, characterized in that: From the 5CrNiMo mold steel substrate outward, there are the first spray layer and the second spray layer, the first coating is a composite spray layer of Cr3C2 and NiCr, and the second coating is a composite spray layer of Cr2O3 and Nano-TiO2; the preparation method steps are as follows: (1) Coating composition ratio: Cr3C2, NiCr, Cr2O3, and Nano-TiO2 particles are used as raw materials, and the content of each component is weighed according to the established composition; (2) Substrate treatment: Cut the hot working die steel into blocks of a predetermined size, clean them with acetone and alcohol to remove oil stains, clean and blow dry, and then polish them layer by layer with 200, 400, 600, 800, and 1000 mesh sandpaper. Then, perform sandblasting. Use suction sandblasting, select 75 mesh brown corundum sand, the sandblasting angle is 60°, the relative moving speed of the spray gun / workpiece is 40m / min, the air pressure is 0.5MPa, and the sandblasting distance is 300mm, in preparation for the next spraying process; (3) Mixing: weighed Cr3C2 and NiCr powders in a ratio of 4:1 are put into anhydrous ethanol and stirred evenly. After ultrasonic oscillation for 5 min, the mixture is kept at 60 °C in a vacuum furnace for 2 h to obtain evenly mixed powder particles. (4) Adding materials: Add the mixed Cr3C2-NiCr powder into the plasma spraying equipment to prepare for spraying processing; (5) Plasma spraying treatment of the first spray layer: The Cr3C2-NiCr coating is sprayed on the surface of 5CrNiMo hot working die steel by plasma spraying technology. The spraying current is 515A, the spraying voltage is 55V, the argon flow rate is 40L / min, the hydrogen flow rate is 3~6L / min, the powder feeding rate is 40g / min, the spraying distance is 120~150m, the spray gun translation rate is 200mm / s, and the spraying is repeated 4 times to obtain a high wear-resistant coating with excellent interlayer bonding and dense structure, namely the first spray layer; (6) Mixing: Weighed Cr2O3 and Nano-TiO2 powders are put into anhydrous ethanol at a ratio of 4:1 and stirred evenly. After ultrasonic oscillation for 7 minutes, the mixture is kept at 70°C in a vacuum furnace for 1.5 hours to obtain uniformly mixed powder particles. Finally, the uniformly mixed powder particles are added to the plasma spraying equipment to prepare for spraying processing. (7) Plasma spraying treatment of the second spray layer: Plasma spraying technology is used to further spray Cr2O3 and Nano-TiO2 composite coating on the surface of Cr3C2-NiCr coating of 5CrNiMo hot working die steel. The spraying current is 515A, the spraying voltage is 55V, the argon flow rate is 40L / min, the hydrogen flow rate is 3~6L / min, the powder feeding rate is 40g / min, the spraying distance is 120~150m, the spray gun translation rate is 200mm / s, and the spraying is repeated 4 times to obtain a self-lubricating gradient wear-resistant component coating, i.e., the second spray layer.

2. The heat-resistant and wear-resistant coating for the mold steel for the steering knuckle according to claim 1, characterized in that: The thickness of the first sprayed layer and the second sprayed layer are both 150-200 μm.

3. A method for preparing a heat-resistant and wear-resistant coating of a mold steel for a steering knuckle according to claim 1 or 2, characterized in that: The preparation steps are as follows: (1) Coating composition ratio: Cr3C2, NiCr, Cr2O3, and Nano-TiO2 particles are used as raw materials, and the content of each component is weighed according to the established composition; (2) Substrate treatment: Cut the hot working die steel into blocks of a predetermined size, clean them with acetone and alcohol to remove oil stains, clean and blow dry, and then polish them layer by layer with 200, 400, 600, 800, and 1000 mesh sandpaper. Then, perform sandblasting. Use suction sandblasting, select 75 mesh brown corundum sand, the sandblasting angle is 60°, the relative moving speed of the spray gun / workpiece is 40m / min, the air pressure is 0.5MPa, and the sandblasting distance is 300mm, in preparation for the next spraying process; (3) Mixing: weighed Cr3C2 and NiCr powders in a ratio of 4:1 are put into anhydrous ethanol and stirred evenly. After ultrasonic oscillation for 5 min, the mixture is kept at 60 °C in a vacuum furnace for 2 h to obtain evenly mixed powder particles. (4) Adding materials: Add the mixed Cr3C2-NiCr powder into the plasma spraying equipment to prepare for spraying processing; (5) Plasma spraying treatment of the first spray layer: The Cr3C2-NiCr coating is sprayed on the surface of 5CrNiMo hot working die steel by plasma spraying technology. The spraying current is 515A, the spraying voltage is 55V, the argon flow rate is 40L / min, the hydrogen flow rate is 3~6L / min, the powder feeding rate is 40g / min, the spraying distance is 120~150m, the spray gun translation rate is 200mm / s, and the spraying is repeated 4 times to obtain a high wear-resistant coating with excellent interlayer bonding and dense structure, namely the first spray layer; (6) Mixing: Weighed Cr2O3 and Nano-TiO2 powders are put into anhydrous ethanol at a ratio of 4:1 and stirred evenly. After ultrasonic oscillation for 7 minutes, the mixture is kept at 70°C in a vacuum furnace for 1.5 hours to obtain uniformly mixed powder particles. Finally, the uniformly mixed powder particles are added to the plasma spraying equipment to prepare for spraying processing. (7) Plasma spraying treatment of the second spray layer: Plasma spraying technology is used to further spray Cr2O3 and Nano-TiO2 composite coating on the surface of Cr3C2-NiCr coating of 5CrNiMo hot working die steel. The spraying current is 515A, the spraying voltage is 55V, the argon flow rate is 40L / min, the hydrogen flow rate is 3~6L / min, the powder feeding rate is 40g / min, the spraying distance is 120~150m, the spray gun translation rate is 200mm / s, and the spraying is repeated 4 times to obtain a self-lubricating gradient wear-resistant component coating, i.e., the second spray layer.