A carbon-rich material synthesized based on a eutectic system and a synthesis method thereof

By synthesizing carbon-rich materials under mild conditions using a eutectic solvent system, the safety and environmental issues of high-temperature and high-pressure hydrothermal carbonization have been solved, achieving an efficient and environmentally friendly preparation method.

CN116119648BActive Publication Date: 2024-11-05NANJING NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310151072.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-11-05
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Existing technologies for preparing carbon-rich materials involve high-temperature and high-pressure hydrothermal carbonization processes that pose safety and environmental problems, and biomass has low reaction efficiency in the solid state.

Method used

A eutectic solvent system (DESys) was used to mix carbohydrate compounds with hydrogen bond acceptors and hydrogen bond donors to form a homogeneous solution. Carbon-rich materials were synthesized under mild conditions and obtained by heating and centrifugation.

Benefits of technology

This method enables the efficient synthesis of carbon-rich materials under mild conditions, reducing energy consumption and environmental pollution, and providing a sustainable preparation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116119648B_ABST
    Figure CN116119648B_ABST
Patent Text Reader

Abstract

The present invention provides a carbon-rich material synthesized based on a low eutectic system and a synthesis method thereof, belonging to the technical field of chemical synthesis. The method comprises the following steps: S1: adding a saccharide compound to a low eutectic solvent aqueous solution to form a mixed solution, wherein the low eutectic solvent comprises a hydrogen bond acceptor and a hydrogen bond donor, and the weight fraction ratio of each component is saccharide compound: hydrogen bond donor: hydrogen bond acceptor: water = 1: (0.7-2.4): (2.5-12.8): (2.2-12.2); S2: heating the mixed solution obtained in step S1 in a magnetic stirrer for a period of time; S3: centrifuging the product of step S1 to remove the lower layer of solid, and drying to obtain a carbon-rich material. The present invention is not only simple to operate and low in cost, but also reduces environmental pollution and is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical synthesis, and in particular relates to a carbon-rich material synthesized based on a low eutectic system and a synthesis method thereof. Background Art

[0002] In recent years, carbon-rich materials have been widely used as solid fuels, heterogeneous catalysis, pollution adsorption, electrochemical energy storage and other applications due to their diverse morphologies and unique properties. Recently, due to environmental issues and the need for sustainable development, many researchers have devoted themselves to finding sustainable resources to prepare carbon-rich materials. Biomass is one of the most abundant renewable resources, which can be converted into carbon-rich materials through thermochemical and biological processes. In the process of producing carbon-rich materials from biomass, complex chemical reactions such as dehydration, decarboxylation, decarboxylation and depolymerization usually occur. In this process, the reaction temperature is crucial to control the main reactions and obtain the desired products, and some of these reactions usually occur simultaneously. Pyrolysis and hydrothermal carbonization (HTC) are the two main methods used to prepare carbon-rich materials from biomass. Compared with slow pyrolysis, hydrothermal carbonization is a more environmentally friendly process because it requires lower temperatures and lower energy consumption.

[0003] The HTC process is carried out under subcritical water pressure below 300 °C. However, the temperature and pressure used in HTC are still high, requiring special equipment, and causing safety and environmental issues for operators. When hydrogen bond donors (HBDs) and hydrogen bond acceptors (HBAs) are mixed to form a deep eutectic system (DESys), the deep eutectic solvent (DES) lowers the melting point of the solvent system by forming hydrogen bonds. We found that plant polysaccharides, a widely available biomass, can be used to prepare carbon-rich materials under mild conditions in a deep eutectic system (DESys) containing oxalic acid, which provides a sustainable method for preparing carbon-rich materials. Unlike DES, the target compound in DESys is regarded as an HBD or HBA, not just another solute. Since part of the biomass and reactants are solid, it is difficult to achieve efficient reactions in the solid state. However, by forming DESys, these biomass and reactants form a homogeneous solution, and some difficult reactions can be achieved under milder conditions. Summary of the invention

[0004] To solve the above problems, the present invention discloses a carbon-rich material synthesized based on a low eutectic system and a synthesis method thereof, which is more environmentally friendly than the previously used methods.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] The present invention first provides a method for synthesizing a carbon-rich material based on a eutectic system, the method comprising the following steps:

[0007] S1: adding a saccharide compound to an aqueous solution of a low eutectic solvent to form a mixed solution, wherein the low eutectic solvent comprises a hydrogen bond acceptor and a hydrogen bond donor, and the weight fraction ratio of each component is saccharide compound: hydrogen bond donor: hydrogen bond acceptor: water = 1: (0.7-2.4): (2.5-12.8): (2.2-12.2);

[0008] S2: heating the mixed solution obtained in step S1 in a magnetic stirrer for a period of time;

[0009] S3: Centrifuge the product of step A to remove the solid layer, and dry it to obtain the carbon-rich material.

[0010] Furthermore, the hydrogen bond acceptors in the low eutectic solvent are all choline chloride, and the hydrogen bond donors in the low eutectic solvent are one or a combination of two or more of oxalic acid, malic acid, lactic acid, and citric acid.

[0011] Furthermore, the heating temperature in step S2 is 80-130 degrees, and the synthesis time is 30-70 minutes.

[0012] Furthermore, the carbohydrate compound includes one or a combination of two or more of plant polysaccharides, monosaccharides, disaccharides, and artificially synthesized polysaccharides.

[0013] The invention also provides a carbon-rich material synthesized based on a low eutectic system.

[0014] The beneficial effects of the present invention are:

[0015] The present invention uses sugar compounds to synthesize carbon-rich materials, aiming to provide new ideas for the sustainable preparation of carbon-rich materials based on low eutectic systems and new solvents that promote reactions. The present invention is not only simple to operate and low in cost, but also reduces environmental pollution and is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 . FTIR spectra of plant polysaccharides and carbon-rich materials in the embodiments of the present invention;

[0017] Figure 2 . Solids of plant polysaccharides and carbon-rich materials in the embodiments of the present invention 13 C-NMR spectroscopy;

[0018] Figure 3 Thermogravimetric spectra of plant polysaccharides and carbon-rich materials in the embodiments of the present invention;

[0019] Figure 4 . The water contact angle diagram of the plant polysaccharide and the carbon-rich material in the embodiment of the present invention, wherein (a) the water contact angle diagram of the plant polysaccharide, (b) the water contact angle diagram of the carbon-rich material;

[0020] Figure 5. The extraction effect of different types of hydrogen bond acceptors on polysaccharides in Dendrobium officinale in the embodiments of the present invention;

[0021] Figure 6 . The effect of the amount of choline chloride added in the embodiment of the present invention on the polysaccharide extraction rate in Dendrobium officinale;

[0022] Figure 7 . The effect of the amount of water added in the embodiment of the present invention on the polysaccharide extraction rate in Dendrobium officinale;

[0023] Figure 8 . The effect of ball milling time on the polysaccharide extraction rate in Dendrobium officinale in the embodiment of the present invention;

[0024] Fig. 9 .The effect of the ball mill rotation speed in the embodiment of the present invention on the polysaccharide extraction rate in Dendrobium officinale. DETAILED DESCRIPTION

[0025] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0026] Example 1

[0027] Synthesis of carbon-rich materials using polysaccharides and deep eutectic solvents

[0028] (1) Preparation of deep eutectic solvent

[0029] Choline chloride and oxalic acid were heated and stirred at 90° C. until they became a homogeneous phase, and then the deep eutectic solvent was diluted with water to 40 wt %.

[0030] (2) Synthesis of polysaccharide-based carbon-rich materials

[0031] 0.6 g of polysaccharide and 10 ml of low eutectic solvent aqueous solution were heated in a magnetic stirrer at 120 degrees and 400 revolutions per minute for 50 minutes, and then the lower layer of solid was removed by centrifugation and dried to obtain a carbon-rich material.

[0032] (3) Characterization and analysis of carbon-rich materials

[0033] When the obtained plant polysaccharide (DOP) was carboxylated using DESys containing oxalic acid, the DESys of oxalic acid / ChCl / polysaccharide released a large amount of gas and produced a black precipitate when heated (120°C). Therefore, we considered whether the polysaccharides in DESys undergo carbonization reaction to generate carbon-rich materials. To confirm this, the black precipitate (DESysChar) was systematically characterized. The elemental analysis results showed that the carbon and oxygen contents of the polysaccharide were 37.0 and 55.2wt%, respectively, while the carbon and oxygen contents of the black precipitate were 50.8 and 36.9wt%, respectively, which were similar to hydrogen char, indicating that the polysaccharide reacted to generate carbon-rich materials.

[0034] The black material was characterized by FTIR spectroscopy, and the results are as follows: Figure 1 As shown. FTIR spectrum shows that the polysaccharide has a -1 There is an absorption peak at 2930, 1740 and 1160 cm-1, corresponding to the OH stretching vibration. -1 The peaks at 1150cm correspond to the CH antisymmetric stretching vibration of the methylene group, the C=O stretching vibration of the ester group, and the asymmetric COC stretching vibration of the polysaccharide. -1 The stretching vibrations near the polysaccharide CO, 810 cm -1 The weak absorption peak near 660cm indicates that the polysaccharide contains phosphate groups. -1 The weak absorption peak near 1712 cm -1 The new peak at 1313 cm represents the C=O stretching vibration of the carboxyl group, indicating that the polysaccharide has been carboxylated. -1 The peak at corresponds to OH or OR attached to aromatic groups, indicating that the polysaccharide may have been dehydrated to form aromatic groups.

[0035] When using solid 13 When DESysChar was characterized by C-NMR, saturated aliphatic groups (δ0-60 ppm), alcohol or ether groups (δ60-105 ppm), furan (δ105-160 ppm), ester or carboxylic acid groups (δ160-185 ppm) and ketone or aldehyde groups (δ185-205 ppm) were found in the spectrum, e.g. Figure 2 Comparing the spectra of DOP and DESysChar, there are no characteristic peaks of aromatic, ester and carboxyl groups in the spectrum of DOP, indicating that the carboxyl and aromatic functional groups are formed through etherification, esterification and dehydration reactions during the formation of DESysChar.

[0036] The DESysChar was characterized by thermogravimetric analysis. Figure 3 It can be seen that the thermal decomposition temperature of DOP is about 210℃, while the decomposition temperature of DESysChar is 193℃. Compared with the thermogravimetric curve of DOP, the thermogravimetric curve of DESysChar decreases slowly, which may be due to multiple reactions during the decomposition of DESysChar. The residual mass of DESysChar is greater than that of DOP, which may be due to the high carbon content of DESysChar.

[0037] Analysis of the hydrophilicity of DESysChar showed that the water contact angle of DESys was similar to that of DOP, such as Figure 4As far as we know, this may be because although the carbon content of DESysChar is relatively high, the presence of hydrophilic functional groups such as carboxyl groups on the surface does not change the hydrophilicity of DESysChar. In addition, when water drops on the surface of DOP, they can adhere to the surface for a while, while when water drops on DESysChar, they quickly penetrate DESysChar. This is because, compared with DOP, DESysChar is granular, which makes it easier for water to penetrate.

[0038] In summary, the present invention directly applies polysaccharides and low eutectic solvents to the synthesis of carbon-rich materials. The invention has obvious advantages in the sample synthesis stage. The whole process requires simple operations, low costs, does not cause additional pollution to the environment, is safe and green, and has broad development prospects in synthesis.

[0039] Embodiment 2:

[0040] The difference between this embodiment and embodiment 1 is that the hydrogen bond donor in this embodiment uses malic acid, lactic acid or citric acid instead of oxalic acid in embodiment 1, and the rest is the same as embodiment 1.

[0041] Embodiment 3:

[0042] The difference between this embodiment and embodiment 1 is that the carbohydrate compound in this embodiment uses polysaccharide, monosaccharide or disaccharide to replace the plant polysaccharide in embodiment 1, and the rest is the same as embodiment 1.

[0043] Embodiment 4:

[0044] The difference between this embodiment and embodiment 1 is that the carbohydrate compound in this embodiment is a polysaccharide extracted from Dendrobium officinale by using the principle of a low eutectic system combined with a ball milling extraction method. The specific extraction method is as follows:

[0045] (1) Extraction of polysaccharides from Dendrobium officinale

[0046] 2 g of Dendrobium officinale powder and 20-40 ml of hydrogen bond acceptor aqueous solution were put into a ball mill, and the ball milling was performed for 10-50 minutes, and then the supernatant was obtained by centrifugation. The plant polysaccharide obtained after ethanol precipitation was quantified by sulfuric acid-phenol method.

[0047] (2) Selection of hydrogen bond acceptors

[0048] Different hydrogen bond acceptors have different hydrogen bond strengths with polysaccharides, and their extraction efficiencies are also different. In order to select the best hydrogen bond acceptor, the present invention studied the extraction rates of different hydrogen bond acceptors. The synthetic raw materials and ratios are shown in Table 1. The results are as follows Figure 5 As shown, it can be seen that the extraction rate of polysaccharides is best when choline chloride is used as the hydrogen bond acceptor.

[0049] Table 1:

[0050]

[0051] (3) Effect of choline chloride amount on extraction

[0052] The present invention explores the extraction effect of choline chloride in an amount of 0.01-0.09 mol. Figure 6 It can be seen that when the amount of choline chloride added is 0.05 mol, the extraction effect is the best. This is because at the beginning, ChCl is continuously added to Dendrobium officinale, and the hydroxyl groups of crude sugar in Dendrobium officinale form hydrogen bonds with the chloride ions in ChCl. The more free chloride ions there are, the easier it is to form more DES, and the more sugar is extracted. When the amount of choline chloride added is 0.05 mol, the hydroxyl groups also basically form hydrogen bonds with ChCl. When more ChCl is added, the viscosity of the entire system will increase, hindering the formation of hydrogen bonds between polysaccharides and ChCl, resulting in a decrease in the amount of extraction. Therefore, the amount of choline chloride added is 0.05 mol.

[0053] (4) Effect of water addition on extraction rate

[0054] Because the viscosity of the system solution is high, it will affect the extraction effect, so water needs to be added for dilution. The present invention explores the extraction effect of adding 20-40 ml of water. Figure 7 It can be seen that when the amount of water added is 30 ml, the extraction effect is the best. This may be because as the amount of water increases, more Dendrobium officinale is added to the reaction process. When the amount of water added reaches a certain amount, all the Dendrobium officinale is fully moistened and added to the reaction, and all the reactants are diluted due to the continuous increase in water volume, causing the amount of sugar extraction to begin to decrease. Therefore, 30 ml of water is selected.

[0055] (5) Effect of ball milling time on extraction

[0056] Too short a ball milling time will result in insufficient dissolution of the cell wall and a reduced extraction rate, while too long a ball milling time will result in too high a solution temperature, which may lead to the decomposition of polysaccharides and reduce the extraction rate, and consume a lot of time. The present invention studies the effect of 10-50 minutes of microwave time on the extraction rate. Figure 8 It can be seen that the ball milling time is most suitable when it is 20 minutes, so 20 minutes is selected as the ball milling time.

[0057] (6) Effect of ball milling speed on extraction

[0058] The effect of ball mill speed on the extraction of polysaccharides by ball milling was studied in the range of 100-500 rpm. Fig. 9 It can be seen that the extraction rate first increased and then decreased, reaching the highest at 300 rpm, so a ball milling speed of 300 rpm was selected for subsequent studies.

[0059] It should be noted that the above content only illustrates the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.

Claims

1. A method for synthesizing a carbon-rich material based on a eutectic system, characterized in that: The method comprises the following steps: S1: adding a saccharide compound to an aqueous solution of a low eutectic solvent to form a mixed solution, wherein the low eutectic solvent comprises a hydrogen bond acceptor and a hydrogen bond donor, and the weight fraction ratio of each component is saccharide compound: hydrogen bond donor: hydrogen bond acceptor: water = 1: (0.7-2.4): (2.5-12.8): (2.2-12.2); S2: heating the mixed solution obtained in step S1 in a magnetic stirrer for a period of time; S3: Centrifuge the product of step S2 to remove the lower layer of solid, and dry it to obtain a carbon-rich material.

2. A method for synthesizing a carbon-rich material based on a eutectic system according to claim 1, characterized in that: The hydrogen bond acceptors in the deep eutectic solvent are all choline chloride, and the hydrogen bond donors in the deep eutectic solvent are one or a combination of two or more of oxalic acid, malic acid, lactic acid and citric acid.

3. The method for synthesizing a carbon-rich material based on a eutectic system according to claim 1, characterized in that: The heating temperature in step S2 is 80-130 degrees, and the synthesis time is 30-70 minutes.

4. The method for synthesizing a carbon-rich material based on a eutectic system according to claim 1, characterized in that: The carbohydrate compound includes one or a combination of two or more of plant polysaccharides, monosaccharides, disaccharides, and artificially synthesized polysaccharides.

5. A carbon-rich material synthesized by the method for synthesizing a carbon-rich material based on a low eutectic system according to any one of claims 1 to 4.