Dielectric composite material and preparation method thereof, dielectric film and preparation method thereof and application thereof
By using dielectric composite materials with fillers such as linear polypropylene and barium titanate in polymer film capacitors, the problems of low dielectric constant and poor compatibility are solved, and the high dielectric constant and energy storage performance are improved. It is suitable for Film capacitor.
Patent Information
- Application Number
- CN202310147554.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-09
AI Technical Summary
In existing polymer film capacitors, the dielectric constant of bidirectional tensile polypropylene (BOPP) dielectric material is low, which limits its energy storage density. The addition of ceramic fillers with high dielectric constant is poor compatibility with the organic matrix, resulting in the material. Increased dielectric loss, decreased leakage current and breakdown strength.
Linear polypropylene (PP) is used as polymer matrix, barium titanate (BT) ceramic particles and styrene-ethylene-butene-styrene block copolymer (SEBS) rubber particles are added as fillers, and the mixture is kneaded and hot pressed. The molding and stretching process prepares dielectric composite materials and films to improve their dielectric constant and energy storage performance.
It achieves a dielectric film with high dielectric constant, good mechanical processing performance and energy storage performance, and has high charge and discharge efficiency, which is suitable for use in film capacitors.
Smart Images

Figure CN116120667B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer-based energy storage dielectric materials, and in particular, to a dielectric composite material and a preparation method thereof, a dielectric film and a preparation method thereof, and applications of the dielectric film. Background Art
[0002] Dielectric capacitors generally use the polarization of dipoles in the dielectric to store electrical energy and have extremely high power density, that is, ultra-fast charge and discharge rates. Compared with lithium-ion batteries, fuel cells, supercapacitors, etc., dielectric capacitors have the advantages of ultra-high power density, fast charge and discharge speed (microseconds), long cycle life, all-solid-state, environmental friendliness, and high safety. Therefore, dielectric capacitors are widely used in power electronics, hybrid vehicles, smart grids, pulse power supplies, aerospace, oil and gas exploration, and new energy fields. Among them, the polymer dielectric material in the polymer film capacitor has the advantages of low cost, high electrical strength, light weight, good processing performance, and high reliability compared with other dielectric materials (such as ceramics, mica, etc.), and is widely used in power electronics, smart grids, new energy vehicles and other fields.
[0003] At present, the most widely used polymer film capacitor in commercial applications is biaxially oriented polypropylene (BOPP) film as the dielectric material, mainly because BOPP has the advantages of high electrical strength and low dielectric loss. However, the low dielectric constant of BOPP greatly limits its energy storage density (<2J / cm 3 ), affecting its further development. In order to improve the dielectric constant of polypropylene, a common method is to add some ceramic fillers with high dielectric constants to the polymer matrix, such as barium strontium titanate (BST), lead zirconate titanate (PZT) and calcium copper titanate (CCTO). However, the properties of these inorganic fillers and the organic matrix (polymer) are quite different, and the volume fraction of nanoparticles added to the composite material is relatively large, which will have some negative effects on the composite material, such as filler agglomeration in the polymer, poor compatibility of the two phases, increased dielectric loss of the material, increased leakage current, decreased breakdown strength and energy density. Summary of the invention
[0004] Based on this, the purpose of this application is to provide a dielectric composite material and a preparation method thereof, a dielectric film and a preparation method and application thereof. The dielectric composite material of this application has excellent mechanical processing performance, high toughness and easy stretching, and the dielectric film prepared by processing has a large dielectric constant, energy storage performance and high charge and discharge efficiency.
[0005] In a first aspect, the present application provides a dielectric composite material, comprising a polymer matrix and a filler filled in the polymer matrix, wherein the material of the polymer matrix includes linear polypropylene (PP), the filler includes ceramic particles and rubber particles, the ceramic particles include barium titanate (BT), and the rubber particles include styrene-ethylene-butylene-styrene block copolymer (SEBS).
[0006] In a second aspect, the present application provides a method for preparing the dielectric composite material, the method comprising: adding a composite material raw material including material pellets of the polymer matrix, the ceramic particles and the rubber particles into an internal mixer for mixing.
[0007] In a third aspect, the present application provides a dielectric film, wherein the dielectric film is made of the dielectric composite material described in the first aspect of the present application.
[0008] In a fourth aspect, the present application provides a method for preparing the dielectric film, the method comprising:
[0009] S1: hot-pressing the dielectric composite material described in the first aspect of the present application to obtain a sheet;
[0010] S2: stretching the sheet.
[0011] In a fifth aspect, the present application provides an application of the dielectric film in the preparation of a thin film capacitor.
[0012] The dielectric composite material of the present application includes linear PP as a polymer matrix (organic matrix), and introduces BT and SEBS as fillers, so that the composite material has high toughness and is suitable for stretching, and has good mechanical processing performance. In addition, in the provided dielectric film, the linear PP material is used as an organic matrix, so that the film has high electrical insulation performance, and BT is used as an inorganic filler to improve the dielectric constant of the film. On this basis, more importantly, the SEBS rubber introduced into the film can effectively improve the compatibility between the inorganic filler BT and the organic matrix PP. While ensuring that the material meets the stretching requirements, the film not only has higher dielectric properties, but also has better energy storage performance.
[0013] Other features and advantages of the present application will be described in detail in the subsequent detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a scanning electron microscope (SEM) image of the stretched film prepared in Example 1. DETAILED DESCRIPTION
[0015] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0016] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0017] According to a first aspect of the present application, the present application provides a dielectric composite material, comprising a polymer matrix and a filler filled in the matrix.
[0018] In the dielectric composite material of the present application, the material of the polymer matrix includes linear polypropylene, which can be selected from various insulating homopolypropylenes suitable for biaxial stretching.
[0019] In some embodiments, the propylene homopolymer has an isotacticity of 96 to 98% and a melt index of 4.3 to 4.7 cm at 190°C and 5.0 kg. 3 / 10min.
[0020] The linear polypropylene can be obtained commercially, for example, HC312 BF, HC300BF and other products of Borclean.
[0021] In the dielectric composite material of the present application, the ceramic particles include barium titanate. As an inorganic filler, the ceramic particles can be selected from various nano-scale barium titanates. In some embodiments, the particle size of the barium titanate is ≤110 nm.
[0022] In some embodiments, in the dielectric composite material, relative to 100 parts by weight of the linear polypropylene, the content of barium titanate is 10 to 50 parts by weight, for example, 10 parts by weight, 12 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, etc. In order to avoid agglomeration and make the composite material have higher comprehensive performance, preferably, in the dielectric composite material, relative to 100 parts by weight of the linear polypropylene, the content of barium titanate is 25 to 40 parts by weight.
[0023] In the dielectric composite material of the present application, the rubber particles include styrene-ethylene-butylene-styrene block copolymer (SEBS). As an organic filler, the SEBS rubber particles have good compatibility with the polymer matrix and the ceramic particles, thereby improving the compatibility between the two.
[0024] In some embodiments, the mass content of the styrene segment (hard segment) in the styrene-ethylene-butylene-styrene block copolymer (SEBS) is 29-35%, for example, 29%, 30%, 31%, 31.5%, 32% or 33%. The SEBS can be obtained commercially, for example, the product of Kraton Company of the United States with the brand name G1651.
[0025] In some embodiments, in the dielectric composite material, relative to 100 parts by weight of the linear polypropylene, the content of SEBS is 1 to 30 parts by weight, for example, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 6 parts by weight, 8 parts by weight, 10 parts by weight, 12 parts by weight, 15 parts by weight, 16 parts by weight, 18 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, etc. In order to effectively improve the compatibility of the ceramic filler with the polymer matrix while making the composite material have a higher dielectric constant, the content of the styrene-ethylene-butylene-styrene block copolymer is preferably 8 to 20 parts by weight, more preferably 8 to 16 parts by weight.
[0026] According to one embodiment, in the dielectric composite material, the content of barium titanate is 25 to 40 parts by weight, and the content of the styrene-ethylene-butylene-styrene block copolymer is 8 to 20 parts by weight relative to 100 parts by weight of the linear polypropylene.
[0027] In some embodiments, in the dielectric composite material, the total content of the filler is 30 to 50 parts by weight, for example, 30 parts by weight, 32 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 42 parts by weight, 45 parts by weight, or 50 parts by weight, relative to 100 parts by weight of the linear polypropylene.
[0028] According to a second aspect of the present application, the present application provides a method for preparing the dielectric composite material, the method comprising: adding a composite material raw material including material pellets of the polymer matrix, the ceramic particles and the rubber particles into an internal mixer for mixing.
[0029] According to the method of the present application, the two fillers are dispersed in the polymer melt through the mixing to achieve the purpose of uniform dispersion. In order to further avoid aging of the polymer material and uneven dispersion of the filler during mixing, preferably, the mixing temperature is 170-190°C, such as 170°C, 175°C, 180°C, 185°C, 190°C; the rotor speed of the internal mixer is 55-65r / min, such as 55r / min, 60r / min, 65r / min, and the mixing time is 10-15min, such as 10min, 11min, 12min, 13min, 14min, 15min.
[0030] In order to further improve the dispersion uniformity of the filler in the polymer matrix, in a preferred embodiment, the method comprises the following steps:
[0031] 1) mixing the polymer matrix material pellets, the ceramic particles and the rubber particles uniformly to obtain a mixed raw material;
[0032] 2) adding 30-70% (e.g., 40%, 50%, 55%, 60%) of the mixed raw materials into an internal mixer and mixing for 5-8 minutes;
[0033] 3) Add the remaining mixed raw materials into the internal mixer and mix for 5 to 8 minutes.
[0034] In steps 2) and 3), the operating conditions of each mixing are as described above and will not be repeated here.
[0035] In step 1), in order to avoid the influence of impurities such as moisture on the material properties, each component can be dried before preparing the mixed raw material. The drying can be carried out in a vacuum oven, and the drying temperature can be 50 to 70° C., such as 55° C., 60° C., and 65° C.; the drying time can be 8 to 15 hours, such as 9 hours, 10 hours, 11 hours, and 12 hours.
[0036] According to the method of the present application, the internal mixer may be a Haake internal mixer.
[0037] By using the method described in the second aspect of the present application, it is possible to obtain the dielectric composite material in which filler particles are uniformly distributed in the polymer matrix and is suitable for mechanical processing.
[0038] According to a third aspect of the present application, the present application provides a dielectric film, which is made of the dielectric composite material described in the first aspect of the present application. The dielectric stretched film may be a biaxially stretched film.
[0039] In the present application, the thickness of the dielectric film can be determined according to its actual application. In order to be applicable to the dielectric of the film capacitor, in some embodiments, the thickness of the dielectric film is 10 to 30 μm, for example, 10 μm, 12 μm, 13 μm, 15 μm, 18 μm, 20 μm.
[0040] In some embodiments, the dielectric constant of the stretched film of the present application with a thickness of 12 to 15 μm is between 2.8 and 3.2, the room temperature breakdown strength is above 280 MV / m, and the discharge energy density at a field strength of 200 MV / m is 0.54 to 0.76 J / cm 3 , the charging and discharging efficiency is above 90%.
[0041] According to a fourth aspect of the present application, the present application provides a method for preparing the dielectric film, the method comprising:
[0042] S1: hot-pressing the dielectric composite material to obtain a sheet;
[0043] S2: stretching the sheet.
[0044] In step S1, the composite material is formed into a sheet suitable for stretching by the hot pressing molding, wherein the hot pressing molding can make the composite material stretch while being heated and softened, and make it close to the frame of the mold by the applied pressure, so as to obtain a sheet suitable for subsequent stretching.
[0045] According to a specific implementation, the operation process of step S1 includes: placing the block-shaped composite material in a mold for preheating, and then applying pressure for thermoforming. The block-shaped composite material can be fixed on a mold covered with a polyimide film.
[0046] In step S1, the composite material is molten by preheating. The preheating temperature (operating temperature) can be 170-200°C, such as 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, etc. The preheating time can be 2-10 minutes, such as 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes.
[0047] Optionally, the pressure of the hot pressing molding is 8 to 15 MPa, for example, 8 MPa, 9 MPa, 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa, 15 MPa, etc.
[0048] Optionally, the temperature of the hot pressing molding is 180-200°C, for example, 180°C, 185°C, 190°C, 195°C, 200°C, etc.
[0049] In step S1, the preheating temperature and the hot pressing temperature may be the same or different.
[0050] In step S1, the time of the hot pressing can be selected according to the required thickness of the sheet. Usually, the time of the hot pressing can be 5 to 20 minutes, such as 8 minutes, 10 minutes, 12 minutes, 13 minutes, 14 minutes, and 15 minutes.
[0051] According to one embodiment, the thickness of the sheet obtained by the hot pressing is 50-70 μm, for example, 50 μm, 55 μm, 60 μm, 65 μm or 70 μm.
[0052] In step S2, the stretching may be biaxial stretching, by which the sheet can be further stretched to obtain a film that meets the use requirements. From the perspective of improving the dispersibility of the filler, preferably, the stretching is biaxial synchronous biaxial stretching.
[0053] Optionally, the preheating temperature of the biaxial stretching is 135-155°C, for example, 135°C, 140°C, 145°C or 150°C.
[0054] Optionally, the preheating time for the bidirectional synchronous stretching is 20 to 50 minutes.
[0055] Optionally, the stretching temperature of the biaxial synchronous stretching is 140-160°C, for example, 140°C, 145°C, 150°C, 155°C or 160°C.
[0056] Optionally, the stretching rate of the bidirectional synchronous stretching is 5 to 10 cm / min, for example, 5 cm / min, 6 cm / min, 7 cm / min, 8 cm / min, 9 cm / min or 10 cm / min.
[0057] According to a specific embodiment, before performing step S1, the preparation method further includes:
[0058] S0: Preparing the dielectric composite material, wherein the method for preparing the dielectric composite material is as described in the second aspect of the present application and will not be repeated here.
[0059] The method of the present application, by selecting appropriate components, makes the composite material have good machinability and is suitable for stretching. Compared with the traditional method of preparing polymer-based dielectric films by solution method, the method of the present application omits the steps of solution dissolution and solvent volatilization, so it has the characteristics of simple process flow and low equipment price, and is suitable for large-scale production.
[0060] According to the fifth aspect of the present application, the present application provides an application of the dielectric film in the preparation of a film capacitor. The dielectric film of the present application has the characteristics of high dielectric constant, high electrical insulation performance, high charge and discharge efficiency, etc., and is suitable for application in film capacitors to meet the use requirements of capacitors.
[0061] The products of the present application are further described below through examples. The examples are only used to explain the present application and should not be construed as limiting the present application.
[0062] In the following examples and comparative examples,
[0063] The ceramic powder is nano-barium titanate (<100 nm), purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., with the product number B118840.
[0064] SEBS rubber particles were purchased from Kraton Corporation of the United States with a brand number of G1651, and contained 33 wt % of styrene (hard segment).
[0065] The linear polypropylene pellets are propylene homopolymers purchased from Borealis Chemicals Ltd. with a brand name of HC312 BF, a melt index of 4.4 g / 10 min at 190° C. and 5 kg, and an isotacticity of 96%.
[0066] All the above raw materials were dried in a vacuum oven before use.
[0067] Example 1
[0068] 100 g of linear polypropylene pellets, 30 g of barium titanate and 20 g of SEBS rubber particles were stirred and mixed uniformly at room temperature (25° C.) to obtain a mixed raw material.
[0069] Take half of the mixed raw materials and add them to a Hake internal mixer, stir them at 180°C and 60r / min for 6 minutes, then add the remaining mixed raw materials, continue stirring under the stirring conditions for 8 minutes to obtain a dielectric composite material mixture, and cut it into small pieces (mass 20-30g) after cooling.
[0070] Each small piece was placed on a mold covered with a polyimide film, preheated at 180°C for 5 min using a hot press, then heated to 190°C and a pressure of 10 MPa was applied to obtain a square sheet (10 cm×10 cm) with a thickness of 60 μm.
[0071] Preheat the biaxial synchronous stretching machine at 150°C for half an hour, then place the above-mentioned square sheet in the biaxial stretching machine. After fixing, perform synchronous biaxial stretching at 150°C at a rate of 5 cm / min to obtain a biaxially stretched dielectric film (SEBS-20wt% / BT-30wt% / PP) with a thickness of 15 μm. This film is recorded as F1.
[0072] Figure 1 This is the SEM image of the film. It can be seen from the figure that BT nanoparticles can be evenly dispersed on the matrix. It can be seen that the addition of SEBS improves the compatibility between the filler and the matrix.
[0073] Example 2
[0074] 100 g of linear polypropylene pellets, 30 g of barium titanate and 16 g of SEBS rubber particles were stirred and mixed uniformly at room temperature to obtain a mixed raw material.
[0075] Take half of the mixed raw materials and add them to the Hake internal mixer, stir them at 175°C and 65r / min for 5 minutes, then add the remaining mixed raw materials and continue stirring for 7 minutes to obtain the dielectric composite material mixture, which is cut into small pieces (mass 20-30g) after cooling.
[0076] Each small piece was placed on a mold covered with a polyimide film, preheated at 175°C for 5 min using a hot press, then heated to 185°C and a pressure of 9 MPa was applied to obtain a square sheet (10 cm×10 cm) with a thickness of 60 μm.
[0077] The biaxial synchronous stretching machine was preheated at 150°C for half an hour, and then the square sheet was placed in the biaxial stretching machine. After fixing, biaxial synchronous stretching was carried out at 145°C at a rate of 6 cm / min to obtain a biaxially stretched dielectric film (SEBS-16wt% / BT-30% / PP) with a thickness of 15 μm. The film was recorded as F2.
[0078] Example 3
[0079] A biaxially oriented dielectric film was prepared according to the method of Example 1, except that the amount of SEBS rubber particles was adjusted to 12 g, thereby obtaining a biaxially oriented dielectric film (SEBS-12wt% / BT-30wt% / PP) with a thickness of 15 μm, and the film was recorded as F3.
[0080] Example 4
[0081] A biaxially oriented film was prepared according to the method of Example 1, except that the amount of SEBS rubber particles was adjusted to 8 g, thereby obtaining a biaxially oriented dielectric film (SEBS-8wt% / BT-30wt% / PP) with a thickness of 15 μm, and the film was recorded as F4.
[0082] Example 5
[0083] A biaxially oriented film was prepared according to the method of Example 1, except that the amount of SEBS rubber particles was adjusted to 4 g, thereby obtaining a biaxially oriented dielectric film (SEBS-4wt% / BT-30wt% / PP) with a thickness of 15 μm, and the film was recorded as F5.
[0084] Comparative Example 1
[0085] The linear polypropylene pellets were placed on a mold covered with a polyimide film, preheated at 180°C for 5 min using a hot press, then heated to 190°C and a pressure of 10 MPa was applied to obtain a square sheet (10 cm×10 cm) with a thickness of 60 μm.
[0086] The biaxial synchronous stretching machine was preheated at 150°C for half an hour, and then the square sheet was placed in the biaxial stretching machine. After fixing, biaxial synchronous stretching was performed at 150°C at a rate of 5 cm / min to obtain a PP film with a thickness of 15 μm. The film was recorded as D-F1.
[0087] Comparative Example 2
[0088] A biaxially oriented film was prepared according to the method of Example 1, except that SEBS rubber particles were not used in the preparation of the film, thereby obtaining a biaxially oriented dielectric film (BT-30% / PP) with a thickness of 15 μm. This film was recorded as D-F2.
[0089] Comparative Example 3
[0090] A biaxially stretched film was prepared according to the method of Example 1, except that barium titanate powder was not used in the preparation of the film, thereby obtaining a biaxially stretched dielectric film (SEBS-20% / PP) with a thickness of 15 μm. This film was recorded as D-F3.
[0091] Example 6
[0092] 100 g of linear polypropylene pellets, 40 g of barium titanate and 10 g of SEBS rubber particles were stirred and mixed uniformly at room temperature to obtain a mixed raw material.
[0093] Take half of the mixed raw materials and add them to a Hake mixer, stir them at 180°C and 65r / min for 5 minutes, then add the remaining mixed raw materials and continue stirring for 10 minutes to obtain a dielectric composite material mixture, which is then cut into small pieces (mass 20-30g) after cooling.
[0094] Each small piece was placed on a mold covered with a polyimide film, preheated at 180°C for 5 min using a hot press, then heated to 195°C and a pressure of 12 MPa was applied to obtain a square sheet (10 cm×10 cm) with a thickness of 60 μm.
[0095] The biaxial synchronous stretching machine was preheated at 150°C for half an hour, and then the square sheet was placed in the biaxial stretching machine. After fixing, biaxial synchronous stretching was performed at 150°C at a rate of 5 cm / min to obtain a biaxially stretched dielectric film (SEBS10-wt% / BT-40wt% PP) with a thickness of 15 μm. The film was recorded as F6.
[0096] Example 7
[0097] 100 g of linear polypropylene pellets, 25 g of barium titanate powder and 15 g of SEBS rubber particles were stirred and mixed uniformly at room temperature to obtain a mixed raw material.
[0098] Take half of the mixed raw materials and add them to a Hake internal mixer, stir them at 185°C and 65r / min for 5 minutes, then add the remaining mixed raw materials and continue stirring for 8 minutes to obtain a dielectric composite material mixture, which is then cut into small pieces (mass 20-30g) after cooling.
[0099] Each small piece was placed on a mold covered with a polyimide film, preheated at 180°C for 5 min using a hot press, then heated to 195°C and a pressure of 12 MPa was applied to obtain a square sheet (10 cm×10 cm) with a thickness of 60 μm.
[0100] Preheat the biaxial synchronous stretching machine at 150°C for half an hour, then place the above-mentioned square sheet in the biaxial stretching machine. After fixing, perform biaxial synchronous stretching at 150°C at a rate of 5 cm / min to obtain a biaxially stretched dielectric film (SEBS-15wt% / BT-25wt% / PP) with a thickness of 15 μm. This film is recorded as F7.
[0101] Comparative Example 4
[0102] A biaxially stretched film was prepared according to the method of Example 7, except that the SEBS rubber particles were replaced with ethylene propylene diene monomer rubber particles (EPDM, LANXESS, Germany, 6160D) of equal mass, thereby obtaining a biaxially stretched film with a thickness of 15 μm, which was recorded as D-F4.
[0103] Test Case
[0104] The upper and lower surfaces of the stretched films F1 to F7 and D-F1 to D-F4 prepared in the above Examples 1 to 7 and Comparative Examples 1 to 4 were gold-plated using a small ion sputtering apparatus as test electrodes (the gold-plated thickness of the upper and lower surfaces was 50 nm, and the electrode area was 0.1256 cm 2 ), and the dielectric properties of the prepared material were tested.
[0105] 1. Dielectric constant
[0106] The dielectric constant was measured using an impedance analyzer at room temperature.
[0107] 2. Room temperature breakdown strength
[0108] The sample was placed between two upper and lower spherical electrodes soaked in dimethyl silicone oil, and a DC voltage was applied using an electrical breakdown tester (BDJC-50KV Beiguang Precision Instrument Equipment Co., Ltd.) until the sample was broken down, with a voltage increase rate of 0.5 kV / s, using the voltage sag criterion. At least 10 points were taken to draw a Weibull distribution function curve for each sample during the breakdown test, and the breakdown strength value (Eb) was calculated when the cumulative failure probability was 63.2%.
[0109] 3. Energy density and charge and discharge efficiency
[0110] The sample was immersed in dimethyl silicone oil, the test conditions were set, and the electric displacement-electric field intensity (DE) curve of the sample was tested using a ferroelectric tester (Radiant, Precision Multiferroic, USA). The required energy density was obtained by integrating the DE curve on the Y axis. The charge and discharge efficiency is expressed as the percentage of the discharge energy density to the charge energy density.
[0111] The test results are shown in Table 1.
[0112] Table 1
[0113]
[0114]
[0115] It can be seen from Table 1 that the films prepared in Examples 1-7 have both higher dielectric constants and more outstanding energy storage performance compared to the films prepared in Comparative Examples 1-4. Among them, compared with Comparative Examples 2 and 3, it can be seen that when SEBS is not introduced as a modified particle in the film, the charge and discharge efficiency performance is poor, and when barium titanate is not introduced, the dielectric constant performance is poor.
[0116] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0117] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A dielectric composite material, characterized in that: The invention comprises a polymer matrix and a filler filled in the polymer matrix, wherein the material of the polymer matrix is linear polypropylene, the filler comprises ceramic particles and rubber particles, the ceramic particles comprise barium titanate, and the rubber particles comprise styrene-ethylene-butylene-styrene block copolymer; The linear polypropylene is a propylene homopolymer with an isotacticity of 96-98% and a melt index of 4.3-4.7 cm at 190°C and 5.0 kg. 3 / 10min; and in the dielectric composite material, relative to 100 parts by weight of the linear polypropylene, the content of barium titanate is 25 to 40 parts by weight, the content of the styrene-ethylene-butylene-styrene block copolymer is 1 to 30 parts by weight, the total content of the filler is 30 to 50 parts by weight, and the mass content of the styrene segment in the styrene-ethylene-butylene-styrene block copolymer is 29 to 35%; The particle size of the barium titanate is less than 100 nm.
2. A method for preparing the dielectric composite material according to claim 1, characterized in that: The method comprises: adding a composite material raw material including a material pellet containing the polymer matrix, the ceramic particles and the rubber particles into an internal mixer for mixing.
3. The method according to claim 2, characterized in that The mixing temperature is 170-190° C., the rotor speed of the internal mixer is 55-65 r / min, and the mixing time is 10-15 min.
4. A dielectric film, characterized in that: The dielectric film is made of the dielectric composite material according to claim 1.
5. The dielectric film according to claim 4, characterized in that: The thickness of the dielectric film is 10-30 μm.
6. A method for preparing the dielectric film according to claim 4 or 5, characterized in that: The preparation method comprises: Hot-pressing the dielectric composite material according to claim 1 to obtain a sheet; The sheet is stretched.
7. The preparation method according to claim 6, characterized in that: The temperature of the hot pressing molding is 180-200° C., and the pressure is 8-15 MPa.
8. The preparation method according to claim 6 or 7, characterized in that: The stretching is bidirectional synchronous bidirectional stretching, the preheating temperature of the bidirectional synchronous stretching is 135-155° C., the stretching temperature is 140-160° C., and the stretching rate is 5-10 cm / min.
9. Use of the dielectric film according to claim 4 or 5 in preparing a film capacitor.