A plasma hydrogenation catalyst and its preparation method and application
The plasma hydrogenation catalyst with tailored composition and preparation enhances the selectivity and efficiency of methane conversion to acrylic acid, addressing resource constraints and process inefficiencies in existing technologies.
Patent Information
- Application Number
- CN202111567213.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-12-20
AI Technical Summary
The existing methods for synthesizing acrylic acid face challenges due to the increasing cost of petroleum resources and water scarcity in coal-rich regions, limiting the efficiency and economic viability of current production processes, while plasma technology offers a promising but inefficient conversion of natural gas into acrylic acid.
A plasma hydrogenation catalyst is developed with a specific composition and preparation method, incorporating a carrier and active component elements like Pt, Rh, Pd, Ir, and auxiliary elements like K, Na, Ca, to enhance the selectivity and efficiency of methane conversion to acrylic acid.
The catalyst achieves high selectivity and efficiency in converting natural gas to acrylic acid at low temperature and normal pressure, reducing costs and adapting to varying gas compositions, thus improving the economic efficiency of the process.
Smart Images

Figure BDA0003422272200000131
Abstract
Description
Technical Field
[0001] The present invention relates to the field of plasma catalysts, and in particular to a plasma hydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] The development of oil and natural gas has led to the rapid development of fine chemicals. Acrylic acid, as one of the important fine chemical raw materials, is widely used in coatings, building materials, adhesives, textiles, leather, papermaking, oil production and water treatment.
[0003] The main methods for synthesizing acrylic acid include the chloroethanol method, the cyanoethanol method, the high-pressure Reppe and modified Reppe methods, the formaldehyde-acetic acid method, the acrylonitrile hydrolysis method, the ethylene method, the propylene direct oxidation method, the propane oxidation method, and the ethylene oxide method. Among them, the only method for large-scale industrial production of acrylic acid is the two-step oxidation method using propylene as the raw material. The main raw material propylene is obtained from petroleum cracking. With the increasing shortage of petroleum resources, the cost of synthesizing acrylic acid has increased significantly.
[0004] In recent years, in addition to improving the propylene oxidation process, my country has also made certain progress in the research and development of other methods for synthesizing acrylic acid. The non-petroleum route of acetylene hydroxylation to synthesize acrylic acid does not rely on petroleum and is suitable for countries and regions that are poor in oil, rich in gas or rich in coal. my country is poor in oil and rich in coal, and has a huge production capacity of coal-to-calcium carbide. In addition, the tail gas of acetylene produced by the calcium carbide process contains a large amount of CO, which can be used as a raw material for the synthesis of acrylic acid by acetylene hydroxylation. However, coal chemical industry consumes a lot of water and energy in the coal gasification stage. Most coal-rich producing areas are short of water, which seriously restricts the development of acrylic acid produced by the acetylene process.
[0005] At present, with the development of combustible ice and shale gas, natural gas reserves are sufficient, and natural gas conversion and utilization technology has become a hot topic. The process of converting natural gas into acrylic acid has become a new direction of technological development. Plasma converts natural gas, and uses electron collision to activate methane under the action of an electric field, and then free radical collision coupling forms products. The plasma method has the characteristics of simple operation, small device size, high energy density and shortened reaction time. It can realize the conversion of natural gas at a lower temperature and is suitable for occasions of different scales, dispersed layouts and variable production conditions. The conversion of methane using plasma technology can be carried out at room temperature and pressure, the operating conditions are relatively mild, the selectivity of specific products is high, and the product is mainly acetylene.
[0006] Therefore, it is necessary to provide a plasma catalyst suitable for direct conversion of natural gas. Summary of the invention
[0007] The purpose of the present invention is to improve the reaction efficiency of the methane conversion process under the premise of ensuring high selectivity of acrylic acid in methane to olefins.
[0008] The inventors of the present invention have found that the addition of auxiliary elements can change the loading state of the active component metal elements on the catalyst carrier, improve the dispersion of the loaded metal surface, increase the metal surface electrons, and also increase the bimetallic contact surface. In addition, the electron-rich state can weaken the adsorption of the active component metal elements to carbon atoms, strengthen the adsorption of oxygen atoms, and facilitate the carbonylation of acetylene and CO, thereby improving the selectivity of acrylic acid. The improvement of acrylic acid selectivity is conducive to reducing the unit consumption of the product, and thus can improve the economic efficiency of the methane conversion process. In view of this, the solution of the present invention is provided.
[0009] In order to achieve the above-mentioned object, the first aspect of the present invention provides a plasma hydrogenation catalyst, which contains a carrier and an active component element and an auxiliary element supported on the carrier, wherein the carrier is selected from at least one of Al2O3, SiO2, MgO, ZrO2, and molecular sieves, and the active component element includes a first active component element and a second active component element, wherein the first active component element is selected from at least one of Pt, Rh, Pd, and Ir, and the second active component element is selected from at least one of Group VIII non-precious metal elements and Group IB metal elements, and the modified auxiliary element is selected from at least one of K, Na, and Ca;
[0010] Based on the total weight of the catalyst, the content of the first active component element is 0.01-0.12 wt %, the content of the second active component element is 0.1-2 wt %, and the content of the modification aid element is 0.01-0.1 wt %.
[0011] The second aspect of the present invention provides a method for preparing the plasma hydrogenation catalyst described in the first aspect, the method comprising: impregnating the pretreated carrier in an aqueous solution containing a first active component element source, a second active component element source and a modification aid element source, and then drying and calcining the solid obtained after the impregnation.
[0012] The third aspect of the present invention provides the use of the plasma hydrogenation catalyst described in the first aspect in the direct conversion of natural gas.
[0013] The catalyst provided by the present invention has the advantages of small loading, low cost, safety and environmental protection. The catalyst is heated by the heat generated after methane is converted by plasma, and no additional heat source is required to activate the catalyst. It can adapt to the composition change of tail gas caused by unstable discharge in the plasma process, and realizes one-step conversion of natural gas into acrylic acid at low temperature and normal pressure. It has high reaction efficiency while ensuring high selectivity of acrylic acid. DETAILED DESCRIPTION
[0014] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0015] As mentioned above, the first aspect of the present invention provides a plasma hydrogenation catalyst, which contains a carrier and an active component element and an auxiliary element supported on the carrier, wherein the carrier is selected from at least one of Al2O3, SiO2, MgO, ZrO2, and molecular sieves, and the active component element includes a first active component element and a second active component element, wherein the first active component element is selected from at least one of Pt, Rh, Pd, and Ir, and the second active component element is selected from at least one of Group VIII non-precious metal elements and Group IB metal elements, and the modified auxiliary element is selected from at least one of K, Na, and Ca;
[0016] Based on the total weight of the catalyst, the content of the first active component element is 0.01-0.12 wt %, the content of the second active component element is 0.1-2 wt %, and the content of the modification aid element is 0.01-0.1 wt %.
[0017] Preferably, the carrier is selected from at least one of Al2O3, SiO2, and MgO.
[0018] Preferably, the average particle size of the carrier is 3-5 mm, preferably 3-3.5 mm.
[0019] Preferably, based on the total weight of the catalyst, the content of the first active component element is 0.09-0.12 wt % calculated as the element, the content of the second active component element is 0.8-1.2 wt % calculated as the element, and the content of the modification aid element is 0.01-0.05 wt % calculated as the element. The inventors of the present invention have found that the catalyst in this preferred case has a higher selectivity for acrylic acid.
[0020] Preferably, the second active component element is selected from at least one of Ni, Fe, Cu, Ag and Au.
[0021] As mentioned above, the second aspect of the present invention provides a method for preparing the plasma hydrogenation catalyst described in the first aspect, the method comprising: impregnating the pretreated carrier in an aqueous solution containing a first active component element source, a second active component element source and a modification aid element source, and then drying and calcining the solid obtained after the impregnation.
[0022] According to a preferred embodiment of the present invention, the pretreatment step comprises:
[0023] The carrier to be pretreated is subjected to a first drying and a first calcination in sequence to obtain an intermediate I;
[0024] Then, the intermediate I is contacted with a solvent for reaction, and the mixture after the contact reaction is contacted with titanium tetrachloride to obtain a solid which is subjected to a second drying and a second calcination in sequence.
[0025] Preferably, the contact reaction is carried out under ultrasonic conditions, and the ultrasonic conditions at least meet the following conditions: ultrasonic time is 1-3 hours, and ultrasonic frequency is 10KHz-40KHz. More preferably, the ultrasonic conditions at least meet the following conditions: ultrasonic time is 1.5-2 hours, and ultrasonic frequency is 20KHz-25KHz.
[0026] Preferably, the first drying conditions at least meet the following conditions: drying time is 8-12 hours, and drying temperature is 100-120°C.
[0027] Preferably, the first calcination conditions at least meet the following requirements: calcination time is 2-6 hours, calcination temperature is 450-500° C., and heating rate is 1-4° C. / min.
[0028] It should be noted that the heating rate represents the amount of change in temperature per unit time. The timing point of the roasting is when the temperature rises to the set roasting temperature value. The present invention does not particularly limit the heating method, and those skilled in the art can select it in combination with the known technology in the art. The following text of the present invention exemplarily provides a method of heating, which should not be understood by those skilled in the art as limiting the present invention.
[0029] Preferably, the solvent is selected from at least one of anhydrous ethanol, methanol and glycerol.
[0030] Preferably, the usage ratio of the intermediate I to the solvent is 1 g: 10-100 mL.
[0031] Preferably, the weight ratio of the intermediate I to the titanium tetrachloride is 1:1-10.
[0032] According to another preferred embodiment of the present invention, the second drying condition at least satisfies: drying time is 10-15h, and drying temperature is 100-120°C. Preferably, the second drying condition at least satisfies: drying time is 11-12h, and drying temperature is 100-120°C.
[0033] Preferably, the second calcination conditions at least meet the following requirements: calcination time is 4-8h, calcination temperature is 450-500°C, and heating rate is 1-4°C / min. Preferably, the first active component element source is selected from at least one of nitrates, acetates, and chlorides that can provide the first active component element. Exemplarily, the first active component element source can be rhodium nitrate, iridium acetate, chloroplatinic acid, and palladium acetate.
[0034] Preferably, the second active component element source is selected from at least one of nitrates and chlorides that can provide the active second component element. Exemplarily, the second active component element source can be iron nitrate, copper nitrate, silver nitrate, chloroauric acid.
[0035] Preferably, the modification aid element source is selected from at least one of nitrates and chlorides that can provide the modification aid element. Exemplarily, the modification aid element source can be potassium nitrate or sodium chloride.
[0036] Preferably, the impregnation conditions at least meet the following requirements: the impregnation time is 8-12 hours, and the impregnation temperature is 20-30°C.
[0037] Preferably, the drying conditions at least meet the following requirements: drying time is 11-12 hours, and drying temperature is 100-120°C.
[0038] Preferably, the calcination conditions at least meet the following requirements: calcination time is 6-12 hours, calcination temperature is 450-500° C., and heating rate is 1-4° C. / min.
[0039] As mentioned above, the third aspect of the present invention provides the use of the plasma hydrogenation catalyst described in the first aspect in the direct conversion of natural gas.
[0040] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all raw materials are commercially available, the element content is measured by ICP, and the average particle size is measured by a particle size analyzer.
[0041] Carrier:
[0042] Al2O3: purchased from Aladdin Reagent Company, with an average particle size of 3.5 mm.
[0043] SiO2: purchased from Aladdin Reagent Company, with an average particle size of 3.5 mm.
[0044] MgO: purchased from Aladdin Reagent Company, with an average particle size of 3.5 mm.
[0045] The first active component element source:
[0046] Rhodium nitrate: analytical grade, purchased from Aladdin Reagent Company.
[0047] Iridium acetate: analytical grade, purchased from Aladdin Reagent Company.
[0048] Chloroplatinic acid: analytical grade, purchased from Aladdin Reagent Company.
[0049] Second active component element source:
[0050] Ferric nitrate: analytical grade, purchased from Aladdin Reagent Company.
[0051] Copper nitrate: analytical grade, purchased from Aladdin Reagent Company.
[0052] Silver nitrate: analytical grade, purchased from Aladdin Reagent Company.
[0053] Modification additive element source:
[0054] Potassium nitrate: analytical grade, purchased from Aladdin Reagent Company.
[0055] Plasma reactor: See patent document CN109289457A, specifically, the plasma reactor includes a blade sliding arc stabilization system and a reactor:
[0056] The blade sliding arc stabilization system comprises a first DC power supply, a second DC power supply, an inductor, a diode and an electromagnetic relay switch, wherein the first DC power supply is connected in series with the inductor and the diode, the electromagnetic relay switch is connected in series with the second DC power supply, the two series branches are connected in parallel and connected to the two electrodes of the reactor, the positive and negative poles of the two DC power supplies are in the same direction and the negative poles are grounded: the first DC power supply adopts a 1.5kV DC power supply, the second DC power supply adopts a 10kV DC power supply, and the inductor 6 adopts a 30mH inductor; the breakdown voltage is provided by the second DC power supply, and the power supply is maintained by the first DC power supply;
[0057] The reactor comprises an outer cover, two electrodes, two flat magnets and a nozzle; the electrodes are arc-shaped blade electrodes (with a radius of 20 mm), which are arranged on the lower wall plate of the reactor and are placed opposite to each other; the outer cover is a straight quadrangular prism structure with a rectangular cross-section (made of quartz, 45 mm*12 mm*110 mm, with a wall thickness of 2 mm), and two flat magnets are arranged parallel to each other on the outside of the outer cover; the nozzle (with a diameter of 2 mm) is arranged on the lower wall plate of the reactor corresponding to the middle of the two electrodes to spray gas into the reactor, and the nozzle outlet is 10 mm away from the narrowest part of the two electrodes; the upper and lower wall plates of the reactor are made of high-temperature resistant insulating material alumina ceramics, and graphite gaskets are padded between the upper and lower wall plates and the outer cover, and the upper and lower wall plates are pressed tightly by screws and nuts to fix the outer cover.
[0058] Preparation Example 1: Preparation of carrier Z1
[0059] The Al2O3 carrier was placed in an oven at 120°C for drying (i.e., first drying) for 12 h, then placed in a muffle furnace, heated to 450°C at a heating rate of 3°C / min, and then calcined (i.e., first calcination) for 4 h to obtain intermediate I;
[0060] 40 g of the intermediate I was added to 400 mL of anhydrous ethanol and ultrasonicated for 2 h at a frequency of 25 KHz; 80 g of titanium tetrachloride was added dropwise after ultrasonication, and then rotary evaporated to obtain a solid, which was then placed in an oven at 120 ° C. to dry (i.e., the second drying) for 12 h, and then placed in a muffle furnace, and the temperature was raised to 450 ° C at a heating rate of 3 ° C and then calcined (i.e., the second calcination) for 5 h to obtain the pretreated carrier Z1.
[0061] Preparation Example 2: Preparation of carrier Z2
[0062] The Al2O3 carrier was placed in an oven at 100°C for drying (i.e., first drying) for 10 h, then placed in a muffle furnace, heated to 500°C at a heating rate of 4°C / min, and then calcined (i.e., first calcination) for 3 h to obtain intermediate I;
[0063] 40 g of the intermediate I was added to 800 mL of anhydrous ethanol and ultrasonicated for 2 h at a frequency of 20 KHz; 90 g of titanium tetrachloride was added dropwise after ultrasonication, and then rotary evaporated to obtain a solid, which was placed in an oven at 100 ° C. and dried (i.e., the second drying) for 10 h, and then placed in a muffle furnace, heated to 500 ° C. at a heating rate of 4 ° C. / min, and then calcined (i.e., the second calcination) for 6 h to obtain the pretreated carrier Z2.
[0064] Preparation Example 3: Preparation of Catalyst C1
[0065] 40 g of the carrier Z1 prepared in Preparation Example 1 was immersed in a mixed solution for 12 h. The mixed solution contained 1.2 g of rhodium nitrate solution (rhodium content of 5 wt%), 0.7 g of ferric nitrate solution (iron content of 30 wt%), 0.6 g of potassium nitrate solution (potassium content of 2 wt%) and 100 mL of deionized water. The mixture was then rotary evaporated in an 80°C water bath for 4 h and dried in an oven at 120°C for 8 h. The mixture was then placed in a muffle furnace, heated to 450°C at a heating rate of 3°C / min and calcined for 5 h to obtain a catalyst, which was recorded as C1.
[0066] The content of the first active component element rhodium in the catalyst C1 is 0.1 wt %, the content of the second active component element iron is 1 wt %, and the content of the modification aid element potassium is 0.05 wt %.
[0067] Preparation Example 4: Preparation of Catalyst C2
[0068] This preparation example adopts a preparation method similar to that of Preparation Example 3, except that:
[0069] An equal volume of rhodium nitrate solution is replaced with an iridium acetate solution having the same mass concentration of the first active component element to obtain a catalyst, which is recorded as C2.
[0070] The content of the first active component element iridium in the catalyst C2 is 0.12 wt %, the content of the second active component element iron is 1 wt %, and the content of the modification aid element potassium is 0.05 wt %.
[0071] Preparation Example 5: Preparation of Catalyst C3
[0072] This preparation example adopts a preparation method similar to that of Preparation Example 3, except that:
[0073] An equal volume of rhodium nitrate solution was replaced with a chloroplatinic acid solution having the same mass concentration of the first active component element to obtain a catalyst, which was recorded as C3.
[0074] The first active component element platinum in the catalyst C3 contained 0.09 wt %, the second active component element iron contained 1 wt %, and the modification aid element potassium contained 0.05 wt %.
[0075] Preparation Example 6: Preparation of Catalyst C4
[0076] This preparation example adopts a preparation method similar to that of Preparation Example 3, except that:
[0077] The catalyst is obtained by replacing an equal weight of carrier Z1 with carrier Z2, and replacing an equal volume of ferric nitrate solution with a copper nitrate solution having the same mass concentration of the second active component element, and is recorded as C4.
[0078] The content of the first active component element rhodium in the catalyst C4 is 0.1 wt %, the content of the second active component element copper is 1.2 wt %, and the content of the modification aid element potassium is 0.05 wt %.
[0079] Preparation Example 7: Preparation of Catalyst C5
[0080] This preparation example adopts a preparation method similar to that of Preparation Example 3, except that:
[0081] An equal volume of the ferric nitrate solution was replaced with a silver nitrate solution having the same mass concentration of the second active component element to obtain a catalyst, which was recorded as C5.
[0082] The content of the first active component element rhodium in the catalyst C5 is 0.1 wt %, the content of the second active component element silver is 1 wt %, and the content of the modification aid element potassium is 0.06 wt %.
[0083] Preparation Example 8: Preparation of Catalyst C6
[0084] This preparation example adopts a preparation method similar to that of Preparation Example 3, except that:
[0085] The Al2O3 carrier was replaced by SiO2 carrier in equal weight to obtain a catalyst, which was recorded as C6.
[0086] The content of the first active component element rhodium in the catalyst C6 is 0.1 wt %, the content of the second active component element iron is 1 wt %, and the content of the modification aid element potassium is 0.05 wt %.
[0087] Preparation Example 9: Preparation of Catalyst C7
[0088] This preparation example adopts a preparation method similar to that of Preparation Example 3, except that:
[0089] The Al2O3 carrier was replaced by an MgO carrier in equal weight to obtain a catalyst, which was designated as C7.
[0090] The content of the first active component element rhodium in the catalyst C7 is 0.1 wt %, the content of the second active component element iron is 0.8 wt %, and the content of the modification aid element potassium is 0.05 wt %.
[0091] Preparation Example 10: Preparation of Catalyst C8
[0092] This preparation example adopts a preparation method similar to that of Preparation Example 3, except that:
[0093] First, the carrier Z1 is sequentially impregnated in a mixed solution of a rhodium nitrate solution and a ferric nitrate solution, dried and calcined to obtain a carrier Z11;
[0094] Then, the carrier Z11 is sequentially impregnated in a potassium nitrate solution, dried and calcined to obtain a catalyst, which is denoted as C8.
[0095] The content of the first active component element rhodium in the catalyst C8 is 0.1 wt %, the content of the second active component element iron is 1 wt %, and the content of the modification aid element potassium is 0.05 wt %.
[0096] Preparation Example 11: Preparation of Catalyst C9
[0097] This preparation example adopts a preparation method similar to that of Preparation Example 1, except that:
[0098] First, the carrier Z1 is sequentially impregnated in a rhodium nitrate solution, dried and calcined to obtain a carrier Z12;
[0099] Then, the carrier Z12 is sequentially impregnated in a mixed solution of ferric nitrate solution and potassium nitrate solution, dried and calcined to obtain a catalyst, which is recorded as C9.
[0100] The content of the first active component element rhodium in the catalyst C9 is 0.1 wt %, the content of the second active component element iron is 1 wt %, and the content of the modification aid element potassium is 0.05 wt %.
[0101] Comparative Example 1: Preparation of Catalyst DC1
[0102] This comparative example adopts a preparation method similar to that of Preparation Example 3, except that:
[0103] The catalyst is obtained by replacing the carrier Z1 with the carrier Z2 in equal weight, and replacing the equal volumes of rhodium nitrate solution and potassium nitrate solution with the sum of the volumes of the above two solutions and the iron nitrate solution having the same mass concentration of the second active component element, and recorded as DC1.
[0104] The content of the second active component element iron in the catalyst DC1 is 1 wt %.
[0105] Comparative Example 2: Preparation of Catalyst DC2
[0106] This comparative example adopts a preparation method similar to that of Preparation Example 3, except that:
[0107] An equal volume of ferric nitrate solution and an equal volume of potassium nitrate solution are replaced by a rhodium nitrate solution having the same mass concentration of the first active component element as the sum of the volume of the above two solutions to obtain a catalyst, which is recorded as DC2.
[0108] The content of rhodium as the first active component element in the catalyst DC2 is 0.1 wt%.
[0109] Comparative Example 3: Preparation of Catalyst DC3
[0110] This comparative example adopts a preparation method similar to that of Preparation Example 3, except that:
[0111] An equal volume of rhodium nitrate solution and an equal volume of potassium nitrate solution are replaced by an iron nitrate solution having the same mass concentration of the second active component element as the sum of the volume of the above two solutions to obtain a catalyst, which is recorded as DC3.
[0112] The content of the second active component element iron in the catalyst DC3 was 1.1 wt%.
[0113] Comparative Example 4: Preparation of Catalyst DC4
[0114] This comparative example adopts a preparation method similar to that of Preparation Example 3, except that:
[0115] An equal volume of ferric nitrate solution and an equal volume of potassium nitrate solution are replaced by a rhodium nitrate solution having the same mass concentration of the first active component element as the sum of the volume of the above two solutions to obtain a catalyst, which is recorded as DC4.
[0116] The content of rhodium as the first active component element in the catalyst DC4 was 1.1% by weight.
[0117] Comparative Example 5: Preparation of Catalyst DC5
[0118] This comparative example adopts a preparation method similar to that of Preparation Example 4, except that:
[0119] An equal volume of ferric nitrate solution and an equal volume of potassium nitrate solution are replaced by an iridium acetate solution having the same mass concentration of the first active component element as the sum of the volume of the above two solutions to obtain a catalyst, which is recorded as DC5.
[0120] The content of iridium, the first active component element, in the catalyst DC5 is 1.1% by weight.
[0121] Comparative Example 6: Preparation of Catalyst DC6
[0122] This comparative example adopts a preparation method similar to that of Preparation Example 5, except that an equal volume of ferric nitrate solution and an equal volume of potassium nitrate solution are replaced by a chloroplatinic acid solution having the same mass concentration of the first active component element as the sum of the volume of the above two solutions, to obtain a catalyst, which is recorded as DC6.
[0123] The content of platinum as the first active component element in the catalyst DC6 was 1.1% by weight.
[0124] Test Case
[0125] The catalyst (40 g) prepared in the above example was placed in a plasma reactor for reaction, wherein the methane flow rate was 0.5 L / min, the hydrogen flow rate was 1.5 L / min, the carbon monoxide flow rate was 1.5 L / min, the discharge power was 110 W, and the discharge was continued for 1 h to stabilize the reaction. The methane conversion rate, acetylene selectivity and acrylic acid selectivity were calculated. The corresponding process conditions and results are shown in Table 1.
[0126] Methane conversion rate is expressed as: methane conversion rate = (methane import molar amount - methane export molar amount) / methane import molar amount × 100%;
[0127] Acetylene selectivity is expressed as: (acetylene outlet molar amount) × 2 / (methane import molar amount-methane export molar amount) × 100%;
[0128] The selectivity of acrylic acid is expressed as: (acrylic acid outlet molar amount)×3 / (methane inlet molar amount-methane outlet molar amount)×100%.
[0129] (The inlet mole or outlet mole means the mole of gas taken out at the inlet or outlet for one minute after the reaction is balanced.)
[0130] Table 1
[0131]
[0132] Table 1 (continued)
[0133] Preparation Example 9 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Catalyst type C9 DC1 DC2 DC3 DC4 DC5 DC6 Temperature, °C 46 38 41 42 41 48 46 Pressure, MPa 0.17 0.13 0.14 0.20 0.14 0.23 0.21 Methane conversion rate, % 36 33 35 37 34 35 36 Acetylene selectivity, % 15 12 17 11 21 16 19 Acrylic acid selectivity, % 76 35 40 30 49 50 48
[0134] It can be seen from the results in Table 1 that the catalyst provided by the present invention can adapt to the composition change of tail gas after natural gas undergoes plasma reaction, realize one-step conversion of natural gas into acrylic acid at low temperature and normal pressure, and has high reaction efficiency while ensuring high selectivity of acrylic acid.
[0135] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A plasma hydrogenation catalyst, characterized in that The catalyst contains a carrier and an active component element and a modification auxiliary element supported on the carrier, wherein the carrier is selected from at least one of Al2O3, SiO2, MgO, ZrO2 and molecular sieves, the active component element includes a first active component element and a second active component element, the first active component element is selected from at least one of Pt, Rh, Pd and Ir, the second active component element is selected from at least one of Group VIII non-noble metal elements and Group IB metal elements, and the modification auxiliary element is selected from at least one of K and Na; Based on the total weight of the catalyst, the content of the first active component element is 0.01-0.12% by weight, the content of the second active component element is 0.1-2% by weight, and the content of the modification aid element is 0.01-0.1% by weight. The carrier is a pretreated carrier, and the pretreatment step comprises: sequentially performing a first drying and a first calcination on the carrier to be pretreated to obtain an intermediate I; Then, the intermediate I is contacted with a solvent for reaction, and the mixture after the contact reaction is contacted with titanium tetrachloride to obtain a solid which is subjected to a second drying and a second calcination in sequence; the weight ratio of the intermediate I to the titanium tetrachloride is 1:1-10.
2. The catalyst according to claim 1, wherein The carrier is selected from at least one of Al2O3, SiO2, and MgO.
3. The catalyst according to claim 1 or 2, wherein The average particle size of the carrier is 3-5 mm.
4. The catalyst according to claim 1 or 2, wherein Based on the total weight of the catalyst, the content of the first active component element is 0.09-0.12 wt %, the content of the second active component element is 0.8-1.2 wt %, and the content of the modification aid element is 0.01-0.05 wt % based on the total weight of the catalyst.
5. The catalyst according to claim 1 or 2, wherein The second active component element is selected from at least one of Ni, Fe, Cu, Ag and Au.
6. A method for preparing the plasma hydrogenation catalyst according to any one of claims 1 to 5, characterized in that: The method comprises: impregnating the pretreated carrier in an aqueous solution containing a first active component element source, a second active component element source and a modification auxiliary agent element source, and then sequentially drying and calcining the solid obtained after the impregnation.
7. The method according to claim 6, wherein: The contact reaction is carried out under ultrasonic conditions, and the ultrasonic conditions at least meet the following requirements: ultrasonic time is 1-3h, and ultrasonic frequency is 10KHz-40KHz.
8. The method according to claim 7, wherein: The first drying conditions at least meet the following requirements: drying time is 8-12 hours, and drying temperature is 100-120°C.
9. The method according to claim 7, wherein: The first calcination conditions at least meet the following requirements: calcination time is 2-6 hours, calcination temperature is 450-500° C., and heating rate is 1-4° C. / min.
10. The method according to claim 7 or 8, wherein: The solvent is selected from at least one of anhydrous ethanol, methanol and glycerol.
11. The method according to claim 10, wherein: The usage ratio of the intermediate I to the solvent is 1g:10-100mL.
12. The method according to claim 7 or 8, wherein: The second drying conditions at least meet the following requirements: drying time is 10-15 hours, and drying temperature is 100-120°C.
13. The method according to claim 7 or 8, wherein: The second calcination conditions at least meet the following requirements: calcination time is 4-8 hours, calcination temperature is 450-500° C., and heating rate is 1-4° C. / min.
14. The method according to claim 6 or 7, wherein: The first active component element source is selected from at least one of nitrates, acetates, and chlorides that can provide the first active component element.
15. The method according to claim 6 or 7, wherein: The second active component element source is selected from at least one of nitrates and chlorides that can provide the second active component element.
16. The method according to claim 6 or 7, wherein: The modification aid element source is selected from at least one of nitrates and chlorides that can provide the modification aid element.
17. The method according to claim 6 or 7, wherein: The impregnation conditions at least meet the following requirements: the impregnation time is 8-12 hours, and the impregnation temperature is 20-30°C.
18. The method according to claim 6 or 7, wherein: The drying conditions at least meet the following requirements: drying time is 11-12 hours, and drying temperature is 100-120°C.
19. The method according to claim 6 or 7, wherein: The calcination conditions at least meet the following requirements: calcination time is 6-12 hours, calcination temperature is 450-500° C., and heating rate is 1-4° C. / min.
20. Use of the plasma hydrogenation catalyst according to any one of claims 1 to 5 in direct conversion of natural gas.
Citation Information
Patent Citations
Greenhouse gas conversion device and method utilizing magnetic field to strengthen blade gliding arc
CN109289457A
Supported chlorination catalyst, preparation method thereof and method for synthesizing 2,3,6-trichloropyridine
CN109092285A
Catalyst for selective hydrogenation of acetylene into ethylene, and preparation method thereof, and method for selectively hydrogenation of acetylene
CN109718762A
Method for regulating and controlling interaction between metal nanoparticles and carrier by plasma
CN112275284A
Method for producing noble metal carrying photocatalyst particle
JP2014097476A