Wear-resistant bamboo plywood and preparation method thereof

Through the combined impregnation process of the two resin glues, the problem of poor wear resistance of bamboo plywood is solved, which significantly improves its wear resistance and avoids cracking and fracture.

CN116277368BActive Publication Date: 2024-11-15福建省闽清双棱竹业有限公司
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202310223236.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-11-15
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

The existing bamboo plywood has poor wear resistance and is prone to cracking and breaking.

Method used

The combined impregnation process of two resin glues is adopted, and the bamboo material is first soaked with the first resin glue, and then dried in the second resin glue. The second resin glue penetrates into the first resin glue to enhance the wear resistance of the bamboo plywood.

Benefits of technology

It significantly improves the wear resistance of bamboo plywood and enhances its crack and break resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116277368B_ABST
    Figure CN116277368B_ABST
Patent Text Reader

Abstract

The invention provides a wear-resistant bamboo plywood and a preparation method thereof. The preparation method comprises the following steps: mixing and heating 10-15 parts by weight of bamboo charcoal powder, 40-60 parts by weight of benzaldehyde, 38-90 parts by weight of 2,4,6-triaminopyrimidine, 17-29 parts by weight of urea and 10-21 parts by weight of ammonia water to obtain a first resin glue; mixing and heating 60-100 parts by weight of phenol, 15-27 parts by weight of formaldehyde, 24-31 parts by weight of urea and 5-12 parts by weight of ammonia water to obtain a second resin glue; immersing bamboo in the first resin glue, drying at 45-60 DEG C for 50-80 minutes, immersing the dried bamboo in the second resin glue, drying at 55-60 DEG C for 70-110 minutes, and obtaining the bamboo plywood. The resin glue used in the plywood of the present invention is divided into a first resin glue and a second resin glue. The bamboo material is first soaked in the first resin glue of a specific component and then soaked in the second resin glue of a specific component. The second resin glue penetrates into the first resin glue, so that the wear resistance of the prepared bamboo plywood is greatly improved, and the bamboo plywood has excellent wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite boards, in particular to a wear-resistant bamboo plywood and a preparation method thereof. Background Art

[0002] Bamboo plywood is tough, moisture-proof, corrosion-resistant, heat-resistant and cold-resistant, has beautiful texture, and has a simple and elegant national style. Its hardness and strength are much higher than those of wood. It is widely used and can be used as a covering decorative panel for indoor ceilings, walls, doors and other parts.

[0003] At present, the existing bamboo plywood is obtained by immersing bamboo boards into special resin glue, drying and then pressing and molding. The bamboo plywood made by using the existing resin glue has poor wear resistance and is easy to crack and break. Summary of the invention

[0004] The purpose of the present invention is to provide a wear-resistant bamboo plywood and a preparation method thereof, so as to solve the problems of poor wear resistance and easy cracking of the existing bamboo plywood.

[0005] The present invention provides a method for preparing a wear-resistant bamboo plywood, comprising the following steps:

[0006] 10-15 parts by weight of bamboo charcoal powder, 40-60 parts by weight of benzaldehyde, 38-90 parts by weight of 2,4,6-triaminopyrimidine, 17-29 parts by weight of urea and 10-21 parts by weight of ammonia water are mixed and heated to prepare a first resin glue;

[0007] 60-100 parts by weight of phenol, 15-27 parts by weight of formaldehyde, 24-31 parts by weight of urea and 5-12 parts by weight of aqueous ammonia are mixed and heated to prepare a second resin glue;

[0008] The bamboo material is immersed in a first resin glue, and dried at 45-60° C. for 50-80 minutes. The dried bamboo material is immersed in a second resin glue, and dried at 55-60° C. for 70-110 minutes to obtain a bamboo plywood.

[0009] The preparation method of the wear-resistant bamboo plywood proposed by the present invention has the following beneficial effects: the resin glue used in the plywood of the present invention is divided into a first resin glue and a second resin glue, the bamboo material is first soaked in the first resin glue of a specific component, and then soaked in the second resin glue of a specific component, and the second resin glue penetrates into the first resin glue, so that the wear resistance of the prepared bamboo plywood is greatly improved, and the bamboo plywood has excellent wear resistance.

[0010] In addition, the method for preparing the wear-resistant bamboo plywood provided by the present invention may also have the following additional technical features:

[0011] Wherein, the preparation method of the first resin glue comprises the following steps:

[0012] 10-15 parts by weight of bamboo charcoal powder are added to 40-60 parts by weight of benzaldehyde, and then 38-90 parts by weight of 2,4,6-triaminopyrimidine, 17-29 parts by weight of urea and 10-21 parts by weight of ammonia water are added in sequence, stirred evenly, and heated to 70-90° C. to obtain a first resin glue.

[0013] Wherein, the preparation method of the second resin glue comprises the following steps:

[0014] 60-100 parts by weight of phenol and 15-27 parts by weight of formaldehyde are first mixed, and then 24-31 parts by weight of urea and 5-12 parts by weight of ammonia water are added, stirred evenly, and heated to 60-80° C. to obtain a second resin glue.

[0015] Wherein, the bamboo material is bamboo silk, bamboo strips or rolled bamboo slices.

[0016] Among them, the dried bamboo filaments, bamboo strips or rolled bamboo slices are longitudinally assembled in the matching mold of a special cold press and then cold pressed, and then the mold is sent to a curing room for heat curing to make bamboo squares; then the mold is unloaded and the bamboo squares are taken out to make reconstructed bamboo structural materials, or they are further processed through sawing, trimming, mortise and tenoning, polishing, painting and drying to make reconstructed bamboo floors.

[0017] Wherein, the composition of the first resin glue is specifically:

[0018] 13 parts by weight of bamboo charcoal powder, 50 parts by weight of benzaldehyde, 60 parts by weight of 2,4,6-triaminopyrimidine, 21 parts by weight of urea and 15 parts by weight of ammonia water.

[0019] Wherein, the composition of the second resin glue is specifically:

[0020] 80 parts by weight of phenol, 21 parts by weight of formaldehyde, 26 parts by weight of urea and 8 parts by weight of aqueous ammonia.

[0021] Wherein, the bamboo material is immersed in the first resin glue for 3 to 8 minutes.

[0022] Wherein, the bamboo material is immersed in the second resin glue for 4 to 6 minutes.

[0023] Among them, the cold pressing plate includes a central pressing plate located in the middle and annular pressing plates sequentially sleeved outside the central pressing plate; the central pressing plate and the annular pressing plates as well as the two adjacent annular pressing plates can slide up and down and be displaced; the hydraulic push rods are arrayed above the central pressing plate and the annular pressing plates respectively to push the central pressing plate and the annular pressing plates downward; the upper part of the liquid tank is a hollow cylindrical shape and the lower end is a bowl shape; a main piston is provided in the sealing sliding sleeve inside the liquid tank; the main piston divides the liquid tank into an upper liquid chamber and a lower liquid chamber from top to bottom; the upper liquid chamber is filled with water and is provided with an electrode pair; the electrode pair can controllably discharge to act on the water in the upper liquid chamber to produce a liquid-electric effect; the lower liquid chamber is filled with hydraulic oil; one end of a plurality of liquid guide tubes is connected to the lower liquid chamber through the bowl shape at the lower end of the liquid tank, and the other end is connected to the hydraulic push rod.

[0024] Among them, the hydraulic push rod includes a hollow cylindrical cylinder body and an upper end sealing sliding sleeve arranged in the hollow cylindrical cylinder body, and a rod body with a lower end extending out of the cylinder body and fixedly connected to the central pressure plate or the annular pressure plate; the upper end of the rod body and the cylinder body enclose a force-conducting cavity; the sealing sliding sleeve in the force-conducting cavity is provided with a sub-piston; the opposite surfaces of the sub-piston and the rod body are respectively fixed with electromagnets that can control the size of the magnetic force and have the same polarity on the opposite surfaces; the sub-piston divides the force-conducting cavity into an upper hydraulic push cavity and a lower magnetic push cavity.

[0025] Wherein, the rod body is guided by a fixed guide sleeve to slide vertically up and down.

[0026] Among them, the liquid tank is located above the center of the cold pressing plate and is connected to the hydraulic push rod through multiple liquid guide tubes; the length of the liquid guide tube is the straight-line distance from the bottom of the liquid tank to the top of the hydraulic push rod; a spring is connected between the main piston and the liquid tank for resetting the main piston.

[0027] The present invention also provides a wear-resistant bamboo plywood, which is prepared according to the above preparation method.

[0028] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention.

[0029] 1. The resin glue used in the plywood of the present invention is divided into a first resin glue and a second resin glue. The bamboo material is first soaked in the first resin glue of a specific component, and then soaked in the second resin glue of a specific component. The second resin glue penetrates into the first resin glue, so that the wear resistance of the prepared bamboo plywood is greatly improved, and the bamboo plywood has excellent wear resistance.

[0030] 2. The cold pressing plate of the cold pressing machine of the present invention adopts a multi-layer ring structure, which is independently pushed by different hydraulic push rods, cooperates with the same pressure transmitted by the hydraulic oil in the lower liquid chamber, and then cleverly combines the repulsive force between the electromagnets that can be flexibly controlled, thereby realizing controllable step-by-step cold pressing from the inside to the outside of the cold pressed plywood. The relay cold pressing method can make the deformation part of the plywood generated during the cold pressing process move laterally from the center to the outside, thereby improving the thickness accuracy of the plywood after cold pressing, and reducing the problem of large internal stress after cold pressing molding. The molded plywood has a more stable shape, is not easy to bend and deform, and is not easy to repeat in size; and is not prone to problems such as breakage or internal cracks.

[0031] 3. The present invention utilizes the characteristic that the electromagnet can simply control the size of the magnetic force by the size of the current. Under the condition of ensuring the same final pressure, the release speed of the pressure of each laminate and the delay time of complete release are controlled, so that the direction and size of the material flow of the cold-pressed plywood can be controlled to a certain extent. Moreover, the process is smooth and stepless, and no abrupt or cliff changes in pressure will be generated; thus ensuring the orderliness, accuracy and efficiency of the plywood cold pressing process.

[0032] 4. The sleeve structure of the present invention cleverly plays the role of stepless stop, can stabilize the position of the main piston, and can steplessly maintain the pressure of the hydraulic oil in the lower liquid chamber and the upper liquid push chamber, thereby achieving pressure maintenance during the cold pressing process; and the main piston can be restored and the positions of various components of the cold pressing machine can be reset simply by controlling the solenoid valve, and the next cold pressing activity can be completed accurately automatically and quickly. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a process schematic diagram of the present invention;

[0034] Figure 2 It is a structural schematic diagram of the cold press in the present invention under normal conditions;

[0035] Figure 3 It is a schematic diagram of the structure of the cold press during cold pressing in the present invention;

[0036] Figure 4 It is a schematic diagram of the cold pressing plate and the hydraulic push rod in the present invention.

[0037] Description of labels:

[0038] 6. Cold press; 61. Liquid tank; 610. Connecting pipe; 611. Main piston; 612. Upper liquid chamber; 613. Lower liquid chamber; 614. Electrode pair; 615. Sleeve; 616. Outer annular chamber; 617. Inner cylindrical chamber; 618. Top liquid chamber; 619. One-way valve; 620. Solenoid valve; 62. Hydraulic push rod; 621. Cylinder body; 622. Rod body; 624. Sub-piston; 625. Electromagnet; 626. Upper liquid push chamber; 627. Lower magnetic push chamber; 631. Center pressure plate; 632. Annular pressure plate; 64. Liquid guide tube; 65. Spring; 66. Guide sleeve. DETAILED DESCRIPTION

[0039] In order to make the purpose, features and advantages of the present invention more obvious and understandable, the specific embodiments of the present invention will be described in detail with reference to the following description. In these descriptions, some specific embodiments in the embodiments of the present invention are specifically disclosed to represent some ways of implementing the principles of the embodiments of the present invention, but it should be understood that the scope of the embodiments of the present invention is not limited thereto. On the contrary, the embodiments of the present invention include all changes, modifications and equivalents that fall within the spirit and connotation of the appended claims.

[0040] Reference Figure 1 , Example 1

[0041] 10 parts by weight of bamboo charcoal powder, 40 parts by weight of benzaldehyde, 38 parts by weight of 2,4,6-triaminopyrimidine, 17 parts by weight of urea and 10 parts by weight of ammonia water are mixed and heated to prepare a first resin glue;

[0042] 60 parts by weight of phenol, 15 parts by weight of formaldehyde, 24 parts by weight of urea and 5 parts by weight of aqueous ammonia are mixed and heated to prepare a second resin glue;

[0043] The bamboo material is immersed in a first resin glue, dried at 45° C. for 50 minutes, and the dried bamboo material is immersed in a second resin glue, dried at 55° C. for 70 minutes to obtain a bamboo plywood;

[0044] The preparation method of the first resin glue comprises the following steps:

[0045] Add 10 parts by weight of bamboo charcoal powder to 40 parts by weight of benzaldehyde, and then add 38 parts by weight of 2,4,6-triaminopyrimidine, 17 parts by weight of urea and 10 parts by weight of ammonia water, stir evenly, and heat to 70° C. to prepare a first resin glue;

[0046] The preparation method of the second resin glue comprises the following steps:

[0047] 60 parts by weight of phenol and 15 parts by weight of formaldehyde are first mixed, and then 24 parts by weight of urea and 5 parts by weight of ammonia water are added, stirred evenly, and heated to 60° C. to obtain a second resin glue;

[0048] The bamboo material is immersed in the first resin glue for 3 minutes, and in the second resin glue for 4 minutes. The bamboo material is bamboo filaments, bamboo strips or rolled bamboo slices. The dried bamboo filaments, bamboo strips or rolled bamboo slices are longitudinally assembled in a matching mold of a special cold press and then cold-pressed. The mold is then sent to a curing room for heat curing to form bamboo squares. The mold is then removed and the bamboo squares are taken out to form reconstructed bamboo structural materials, or they are further processed through sawing, trimming, mortise and tenoning, polishing, painting and drying to form reconstructed bamboo floors. Example 2

[0049] 15 parts by weight of bamboo charcoal powder, 60 parts by weight of benzaldehyde, 90 parts by weight of 2,4,6-triaminopyrimidine, 29 parts by weight of urea and 21 parts by weight of ammonia water are mixed and heated to prepare a first resin glue;

[0050] 100 parts by weight of phenol, 27 parts by weight of formaldehyde, 31 parts by weight of urea and 12 parts by weight of aqueous ammonia are mixed and heated to prepare a second resin glue;

[0051] The bamboo material is immersed in a first resin glue, and dried at 60° C. for 80 minutes, and the dried bamboo material is immersed in a second resin glue, and dried at 60° C. for 110 minutes to obtain a bamboo plywood;

[0052] The preparation method of the first resin glue comprises the following steps:

[0053] 15 parts by weight of bamboo charcoal powder is added to 60 parts by weight of benzaldehyde, and then 90 parts by weight of 2,4,6-triaminopyrimidine, 29 parts by weight of urea and 21 parts by weight of ammonia water are added in sequence, the mixture is stirred evenly, and the mixture is heated to 90° C. to prepare a first resin glue;

[0054] The preparation method of the second resin glue comprises the following steps:

[0055] 100 parts by weight of phenol and 27 parts by weight of formaldehyde are first mixed, and then 31 parts by weight of urea and 12 parts by weight of ammonia water are added, stirred evenly, and heated to 80° C. to obtain a second resin glue;

[0056] The bamboo material is immersed in the first resin glue for 8 minutes, and in the second resin glue for 6 minutes. The bamboo material is bamboo filaments, bamboo strips or rolled bamboo slices. The dried bamboo filaments, bamboo strips or rolled bamboo slices are longitudinally assembled in a matching mold of a special cold press and then cold-pressed. The mold is then sent to a curing room for heat curing to form bamboo squares. The mold is then removed and the bamboo squares are taken out to form reconstructed bamboo structural materials, or they are further processed through sawing, trimming, mortise and tenoning, polishing, painting and drying to form reconstructed bamboo floors. Example 3

[0057] 13 parts by weight of bamboo charcoal powder, 50 parts by weight of benzaldehyde, 60 parts by weight of 2,4,6-triaminopyrimidine, 22 parts by weight of urea and 15 parts by weight of ammonia water are mixed and heated to prepare a first resin glue;

[0058] 80 parts by weight of phenol, 21 parts by weight of formaldehyde, 28 parts by weight of urea and 10 parts by weight of aqueous ammonia are mixed and heated to prepare a second resin glue;

[0059] The bamboo material is immersed in a first resin glue, dried at 50° C. for 70 minutes, and the dried bamboo material is immersed in a second resin glue, dried at 58° C. for 100 minutes to obtain a bamboo plywood;

[0060] The preparation method of the first resin glue comprises the following steps:

[0061] 13 parts by weight of bamboo charcoal powder is added to 50 parts by weight of benzaldehyde, and then 60 parts by weight of 2,4,6-triaminopyrimidine, 22 parts by weight of urea and 15 parts by weight of ammonia water are added in sequence, the mixture is stirred evenly, and the mixture is heated to 80° C. to prepare a first resin glue;

[0062] The preparation method of the second resin glue comprises the following steps:

[0063] 80 parts by weight of phenol and 21 parts by weight of formaldehyde are first mixed, and then 28 parts by weight of urea and 10 parts by weight of ammonia water are added, stirred evenly, and heated to 70° C. to obtain a second resin glue;

[0064] The bamboo material is immersed in the first resin glue for 5 minutes, and in the second resin glue for 5 minutes. The bamboo material is bamboo filaments, bamboo strips or rolled bamboo slices. The dried bamboo filaments, bamboo strips or rolled bamboo slices are longitudinally assembled in a matching mold of a special cold press and then cold-pressed. The mold is then sent to a curing room for heat curing to form bamboo squares. The mold is then removed and the bamboo squares are taken out to form reconstructed bamboo structural materials, or they are further processed through sawing, trimming, mortise and tenoning, polishing, painting and drying to form reconstructed bamboo floors.

[0065] In summary, the present invention provides a wear-resistant bamboo plywood and a preparation method thereof. The resin glue used in the plywood of the present invention is divided into a first resin glue and a second resin glue. The bamboo material is first soaked in the first resin glue of a specific component, and then soaked in the second resin glue of a specific component. The second resin glue penetrates into the first resin glue, so that the wear resistance of the prepared bamboo plywood is greatly improved, and the bamboo plywood has excellent wear resistance.

[0066] In addition, refer to Figures 2 to 4On the basis of the above embodiment, the cold press machine 6 includes a liquid tank 61, a plurality of hydraulic push rods 62 and a cold press plate; the cold press plate includes a central press plate 631 located in the middle and an annular press plates 632 sequentially sleeved outside the central press plate 631; the central press plate 631 and the annular press plates 632 as well as the adjacent two annular press plates 632 can be slidably displaced up and down; the hydraulic push rods 62 are arranged above the central press plate 631 and the annular press plates 632 respectively to push the central press plate 631 and the annular press plates 632 downward; the upper portion of the liquid tank 61 It is a hollow cylinder with a bowl-shaped lower end; a main piston 611 is provided in a sealed sliding sleeve in the liquid tank 61; the main piston 611 divides the liquid tank 61 into an upper liquid chamber 612 and a lower liquid chamber 613; the upper liquid chamber 612 is filled with water and is provided with an electrode pair 614; the electrode pair 614 can controllably discharge to act on the water in the upper liquid chamber 612 to produce a liquid-electric effect; the lower liquid chamber 613 is filled with hydraulic oil; one end of a plurality of liquid guide tubes 64 is connected to the lower liquid chamber 613 through the bowl-shaped lower end of the liquid tank 61, and the other end is connected to the hydraulic push rod 62.

[0067] Furthermore, the hydraulic push rod 62 includes a hollow cylindrical cylinder body 621 and a sealing sliding sleeve at the upper end arranged in the hollow cylindrical cylinder body 621, and a rod body 622 at the lower end extending out of the cylinder body 621 and fixedly connected to the central pressure plate 631 or the annular pressure plate 632; the upper end of the rod body 622 and the cylinder body 621 enclose a force-conducting cavity; the sealing sliding sleeve in the force-conducting cavity is provided with a sub-piston 624; electromagnets 625 that can control the size of the magnetic force and have the same polarity on the opposite surfaces of the sub-piston 624 and the rod body 622 are respectively fixed; the sub-piston 624 divides the force-conducting cavity into an upper hydraulic push cavity 626 and a lower magnetic push cavity 627.

[0068] Furthermore, the rod body 622 is guided by a fixed guide sleeve 66 to slide vertically up and down.

[0069] Furthermore, electric heating wires are embedded in the central pressing plate 631 and the annular pressing plate 632 ; the central pressing plate 631 and the annular pressing plate 632 are heat-conducting rigid bodies.

[0070] Furthermore, the liquid tank 61 is located above the center of the cold pressing plate and is connected to the hydraulic push rod 62 through multiple liquid guide tubes 64; the length of the liquid guide tubes 64 is the straight-line distance from the bottom of the liquid tank 61 to the top of the hydraulic push rod 62; a spring 65 is connected between the main piston 611 and the liquid tank 61 for resetting the main piston 611.

[0071] Furthermore, a sealable and retractable sleeve 615 is provided in the upper liquid chamber 612; the upper end of the sleeve 615 is fixedly connected to the top of the upper liquid chamber 612, and the lower end is fixedly connected to the main piston 611, and the upper liquid chamber 612 is sealed and separated into an inner cylindrical chamber 617 and an outer annular chamber 616; the electrode pair 614 is arranged in the inner cylindrical chamber 617; a top liquid chamber 618 is arranged above the upper liquid chamber 612; the outer annular chamber 616 is connected to the top liquid chamber 618 through a plurality of one-way valves 619, so that the hydraulic oil in the top liquid chamber 618 can enter the outer annular chamber 616 in one direction through the one-way valve 619; a connecting pipe 610 is also connected between the outer annular chamber 616 and the top liquid chamber 618; and an electromagnetic valve 620 is arranged on the connecting pipe 610.

[0072] For the preparation process of plywood, the cold pressing method is:

[0073] ① Place the bamboo pieces to be cold pressed in the bottom mold, and control the electrode pair 614 to generate a high-voltage strong electric field through the controller. The high-voltage strong electric field generates a liquid-electric effect in the water in the inner cylindrical cavity 617. The impact force generated pushes the main piston 611 to move downward, squeezing the hydraulic oil in the lower liquid cavity 613;

[0074] ② The squeezed hydraulic oil enters the upper hydraulic push chamber 626 through the liquid guide tube 64, pushing the sub-piston 624 to move downward;

[0075] ③ Due to the repulsive effect of the sub-piston 624 and the electromagnet 625 on the rod body 622, as the sub-piston 624 approaches the upper end of the rod body 622, the repulsive force increases until the two touch or the repulsive force is greater than the pressure of the hydraulic oil on the sub-piston 624, the rod body 622 completely receives the hydraulic pressure, and transmits the pressure to the plywood to be formed through the central pressure plate 631 and the annular pressure plate 632; and the repulsive force between the two electromagnets 625 determines the distance that the sub-piston 624 and the rod body 622 can approach and the time when the rod body 622 completely receives the hydraulic pressure. The controller controls the magnetic force of each electromagnet 625 according to the design requirements, and the repulsive force gradually decreases from the central pressure plate 631 to the outside, so that the central pressure plate 631 first squeezes the bamboo slices, and then from the inside to the outside, and the remaining annular pressure plates 632 squeeze the bamboo slices in turn;

[0076] ④ While step ① is being performed, the main piston 611 stretches the sleeve 615 downward during the downward movement, so that the volume of the outer annular cavity 616 increases, generating negative pressure, and the hydraulic oil is sucked in from the top liquid cavity 618 through the one-way valve 619 for filling; due to the presence of the one-way valve 619, the sucked hydraulic oil cannot be discharged by itself, thereby stabilizing the position of the main piston 611, and being able to infinitely maintain the pressure of the hydraulic oil in the lower liquid cavity 613 and the upper liquid push cavity 626, thereby achieving pressure maintenance during the cold pressing process;

[0077] ⑤ After the cold pressing is completed, the solenoid valve 620 is opened through the controller. Under the combined effect of the restoring force of the plywood, the restoring force of the spring 65 and the negative pressure in the inner cylindrical cavity 617, the main piston 611 moves back upward and squeezes the hydraulic oil in the outer annular cavity 616 back into the top liquid cavity 618 through the connecting pipe 610 until the components of the cold press return to their initial positions.

[0078] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing wear-resistant bamboo plywood, It is characterized in that The following steps are involved: 10-15 parts by weight of bamboo charcoal powder, 40-60 parts by weight of benzaldehyde, 38-90 parts by weight of 2,4,6-triaminopyrimidine, 17-29 parts by weight of urea and 10-21 parts by weight of ammonia water are mixed and heated to prepare a first resin glue; 60-100 parts by weight of phenol, 15-27 parts by weight of formaldehyde, 24-31 parts by weight of urea and 5-12 parts by weight of aqueous ammonia are mixed and heated to prepare a second resin glue; The bamboo material is immersed in a first resin glue, dried at 45-60° C. for 50-80 minutes, and the dried bamboo material is immersed in a second resin glue, dried at 55-60° C. for 70-110 minutes to obtain a bamboo plywood; The preparation method of the first resin glue comprises the following steps: adding 10-15 parts by weight of bamboo charcoal powder to 40-60 parts by weight of benzaldehyde, and then sequentially adding 38-90 parts by weight of 2,4,6-triaminopyrimidine, 17-29 parts by weight of urea and 10-21 parts by weight of ammonia water, stirring evenly, heating to 70-90° C., and obtaining the first resin glue; the preparation method of the second resin glue comprises the following steps: firstly mixing 60-100 parts by weight of phenol and 15-27 parts by weight of formaldehyde, and then adding 24-31 parts by weight of urea and 5-12 parts by weight of ammonia water, stirring evenly, and heating to 60-80° C., and obtaining the second resin glue; The bamboo material is bamboo filaments, bamboo strips or rolled bamboo chips; the bamboo plywood is prepared by longitudinally assembling the dried bamboo filaments, bamboo strips or rolled bamboo chips in a matching mold of a special cold press machine and then cold pressing them; then the mold is sent to a curing room for heat curing to form bamboo squares; then the mold is unloaded and the bamboo squares are taken out to form reconstituted bamboo structural materials; The cold press machine (6) comprises a liquid tank (61), a plurality of hydraulic push rods (62) and a cold press plate; the cold press plate comprises a central press plate (631) located in the middle and annular press plates (632) sequentially sleeved outside the central press plate (631); the central press plate (631) and the annular press plates (632) as well as two adjacent annular press plates (632) can slide up and down; the hydraulic push rods (62) are arranged in an array above the central press plate (631) and the annular press plates (632) respectively to push the central press plate (631) and the annular press plates (632) downward; the upper part of the liquid tank (61) is a hollow cylindrical , the lower end is bowl-shaped; a main piston (611) is provided in the sealing sliding sleeve in the liquid box (61); the main piston (611) divides the liquid box (61) into an upper liquid chamber (612) and a lower liquid chamber (613) from top to bottom; the upper liquid chamber (612) is filled with water and is provided with an electrode pair (614); the electrode pair (614) can controllably discharge to act on the water in the upper liquid chamber (612) to generate a liquid-electric effect; the lower liquid chamber (613) is filled with hydraulic oil; one end of a plurality of liquid guide tubes (64) is connected to the lower liquid chamber (613) through the bowl-shaped lower end of the liquid box (61), and the other end is connected to the hydraulic push rod (62).

2. The method for preparing the wear-resistant bamboo plywood according to claim 1, It is characterized in that The ingredients of the first resin glue are specifically: 13 parts by weight of bamboo charcoal powder, 50 parts by weight of benzaldehyde, 60 parts by weight of 2,4,6-triaminopyrimidine, 21 parts by weight of urea and 15 parts by weight of ammonia water; the ingredients of the second resin glue are specifically: 80 parts by weight of phenol, 21 parts by weight of formaldehyde, 26 parts by weight of urea and 8 parts by weight of ammonia water.

3. The method for preparing the wear-resistant bamboo plywood according to claim 1, It is characterized in that The time for the bamboo material to be immersed in the first resin glue is 3 to 8 minutes; the time for the bamboo material to be immersed in the second resin glue is 4 to 6 minutes.

4. The method for preparing the wear-resistant bamboo plywood according to claim 1, It is characterized in that The hydraulic push rod (62) comprises a hollow cylindrical cylinder body (621) and a rod body (622) whose upper end sealing sliding sleeve is arranged in the hollow cylindrical cylinder body (621) and whose lower end protrudes out of the cylinder body (621) and is fixedly connected to a central pressure plate (631) or an annular pressure plate (632); the upper end of the rod body (622) and the cylinder body (621) enclose a force-conducting cavity; the sealing sliding sleeve in the force-conducting cavity is provided with a sub-piston (624); electromagnets (625) capable of controlling the magnitude of magnetic force and having the same polarity on the opposite surfaces of the sub-piston (624) and the rod body (622) are respectively fixed on the opposite surfaces thereof; the sub-piston (624) divides the force-conducting cavity into an upper hydraulic push cavity (626) and a lower magnetic push cavity (627).

5. The method for preparing the wear-resistant bamboo plywood according to claim 4, It is characterized in that The rod body (622) is guided by a fixed guide sleeve (66) to slide vertically up and down.

6. The method for preparing the wear-resistant bamboo plywood according to claim 5, It is characterized in that The liquid tank (61) is located above the center of the cold pressing plate and is connected to the hydraulic push rod (62) through a plurality of liquid guide tubes (64); the length of the liquid guide tubes (64) is the straight-line distance from the bottom of the liquid tank (61) to the top of the hydraulic push rod (62); a spring (65) is connected between the main piston (611) and the liquid tank (61) for resetting the main piston (611).

7. A wear-resistant bamboo plywood, It is characterized in that Wear-resistant bamboo plywood prepared according to the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for manufacturing bamboo plywood

    CN101439532A

  • Preparation method of adhesive special for bamboo products

    CN102206477A

  • Modified phenol formaldehyde resin and preparation method thereof

    CN102690403A

  • High-strength high-wear-resistance plywood and preparation method thereof

    CN105038281A

  • Shock-proof self-cleaning impregnated paper and preparation method thereof

    CN109306246A