A glass through-hole copper electroplating solution for radio frequency devices and copper electroplating process thereof
By using the combination of S1 pulse square wave current and S2 unidirectional DC current in glass through-hole plating technology, the problems of narrow control range and low production efficiency of traditional electroplating solution are solved, and the hole-free filling and efficient production are achieved, ensuring that The uniformity and brightness of copper plating.
Patent Information
- Application Number
- CN202211567798.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-07
AI Technical Summary
Traditional glass through-hole electroplating technology has the problem of narrow control range of electroplating solution and prone to voids and pore metal dissatisfaction. The existing leveling agent and brightener systems are not suitable for high-speed production efficiency, resulting in the plating time and thick surface copper, which increases the Difficulty and process of subsequent grinding and casting.
The center of the hole is filled with the S1 pulse square wave current, and the center of the hole is filled with blind holes through the S2 unidirectional DC current. The filling of the holes is achieved without holes in the same tank liquid through a specific current output method, avoiding the replacement of the electroplating tank liquid and improving production efficiency.
Through-hole metallization without hole filling is achieved, the process flow is reduced, production efficiency is improved, and through the combination of composite accelerator and wetting agent, the copper plating is evenly distributed and delicate and bright, avoiding the generation of holes and joints.
Smart Images

Figure CN116282949B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper electroplating, and in particular to a through-glass copper electroplating solution for radio frequency devices and a copper electroplating process thereof. Background Art
[0002] Through-glass vias (TGVs) have better high-frequency characteristics than through-silicon vias (TSVs) at high frequencies, and glass substrates have lower manufacturing costs and thickness advantages as low as 100μm under large panel manufacturing processes. TGVs in 3D packaging systems (SiPs) with integrated antennas enable wireless in-plane / out-of-plane and in-chip / inter-chip communications. Compared with wired methods, wireless interconnection can reduce signal latency and increase communication distance with almost no dispersion.
[0003] When the traditional copper electroplating liquid formula uses direct current electroplating for through-hole electroplating, the electroplating liquid control range is narrow, and problems such as voids and insufficient hole metal are prone to occur during the through-hole metallization filling process. Some electroplating takes a long time and the surface copper thickness is thick, which increases the difficulty of subsequent grinding and polishing. When pulse electroplating is used, two blind holes are formed at both ends after butterfly filling in the middle of the hole, which cannot be filled further. Generally, the electroplating tank liquid needs to be replaced for blind hole electroplating filling, which increases the process.
[0004] In addition, patent CN111441071A discloses a double-sided copper plating technology for through-glass holes. Due to defects in the leveling agent and brightener system, the current density range is narrow and it is not suitable for high-speed production efficiency. In order to solve the defects of leveling agents and brighteners, manufacturers in the market have also made many efforts. For example, patent CN103924268A discloses the application of an acid copper leveling agent. This type of leveling agent is a quaternary ammonium salt compound, and the anion X=Cl - or Br - , containing one of S or N, alkyl, alkenyl, aralkyl, heteroaralkyl, substituted alkyl, substituted alkenyl, substituted aralkyl or substituted heteroaralkyl, and is mainly used in wafer electroplating with adjustable surface morphology. However, the above-mentioned leveling agent still cannot achieve satisfactory results.
[0005] In view of the above problems, the present invention has developed a new through-hole electroplating solution formula, which can form a state in which the copper in the through-hole is thick and the copper at the hole mouth is thin under appropriate pulse conditions, and the copper protruding in the middle of the hole is used as the starting point for plating the hole-filling solution to form a butterfly wing. Afterwards, the pulse waveform can be changed to achieve the continued filling of the blind hole. It effectively ensures that there is no void filling in the hole while avoiding the production replacement of the electroplating tank, thereby improving production efficiency. Summary of the invention
[0006] In view of the shortcomings of the above-mentioned technologies, the present invention provides a glass through-hole copper plating solution for radio frequency devices and a copper plating process thereof. The technology adopts S1 pulse square wave current to perform preferential nucleation butterfly filling in the middle of the hole and S2 unidirectional direct current to perform blind hole filling deposition, thereby ensuring void-free filling of the through-hole. The metallization of the entire through-hole can be completed by simply setting different current output modes, without the need to replace the plating tank, thereby improving production efficiency.
[0007] To achieve the above object, the present invention provides a through-glass copper plating solution for radio frequency devices, comprising the following mass concentration components:
[0008] Copper methanesulfonate 250-330g / L
[0009] Methanesulfonic acid 15-35g / L
[0010] Chloride ion 40-90mg / L
[0011] Composite accelerator 120-300mg / L
[0012] Wetting agent 10-80mg / L
[0013] Composite leveling agent 20-50mg / L
[0014] Composite nucleating agent 1-8mg / L
[0015] DI pure water balance.
[0016] Temperature 22-26℃
[0017] The chloride ions are provided by hydrochloric acid.
[0018] Among them, the composite accelerator is sodium methylenebis(methylnaphthalene sulfonate) and 5-chloro-2-methyl-4-isothiazoline-3-one, and the mass ratio of the two when used is 5:1. It can be adsorbed on the high potential area on the surface of the through hole, inhibit the growth of copper at the hole mouth and surface, and is conducive to the preferential deposition of copper inside the through hole in the low potential area, thereby achieving an ideal growth pattern.
[0019] The wetting agent is triblock polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F127, whose molecular formula is PEO106-PPO70-PEO106, which is used to reduce the surface tension of the plating solution, increase the uniform distribution effect of the plating solution in the hole, and make the metal copper electroplated and deposited on the seed layer of the through hole in an orderly manner.
[0020] The composite leveler is a compound composed of dithienyl-pyrrolopyrrole dione and sodium carboxymethyl cellulose, and the mass concentration ratio of the two when used is 4:1, which makes the copper plating crystals fine and bright; at the same time, it inhibits copper plating in high current density areas, and works together with other components to achieve an ideal through-hole butterfly filling mode.
[0021] The composite nucleating agent is sodium 5-nitroguaiacol and 6-chloroimidazo[1,2-b]pyridazine, and the mass concentration ratio of the two when used is 1:1, which can assist the additives in adsorbing in different potential zones, play the corresponding acceleration and inhibition leveling functions, and strengthen the preferential nucleation filling of electroplated copper in the middle of the hole in the initial stage.
[0022] A copper electroplating process for through-glass vias of radio frequency devices comprises the following specific steps:
[0023] Step 1: Degrease and clean the through-hole glass plate coated with the corresponding seed layer for 5-10 minutes to remove the oil stains on the surface, and then rinse with DI pure water for 3 times to remove the excess degreaser;
[0024] Step 2: The cleaned through-hole glass plate is fixed on a double-sided electroplating apparatus and immersed in the copper electroplating solution described in any one of claims 1 to 5;
[0025] Step 3, turn on the power supply and apply S1 current, wherein the applied S1 current is a periodic commutation pulse electroplating square wave current with an off time of 10-60ms per cycle;
[0026] In step 4, a S2 current is applied, and the applied current is a unidirectional direct current.
[0027] Among them, the specific conditions of step 3 are: current density 0.5-1.5ASD, plating solution circulation rate 0.5-2TO / h, electroplating time 0.5-1.0h, the forward and reverse current density ratio in each cycle is 1:2-5, and the forward and reverse pulse time ratio is 40-60:1.
[0028] The specific conditions of step 4 are: current density of 2-5ASD, plating solution circulation rate of 3-4TO / h, and electroplating time of 1.0-2.5h.
[0029] In the S1 stage, using pulsed square wave current for electroplating can achieve the effect of slow surface deposition and relatively fast deposition in the hole, so that the electroplated copper first connects in the middle of the through hole to form butterfly wings, and then gradually deposits to the openings on both sides of the through hole, effectively avoiding the formation of holes or gaps in the through hole under other growth modes. In the S2 stage, it is adjusted to unidirectional DC output to continue filling the formed blind hole, thereby completing the metallization filling of the entire through hole.
[0030] The beneficial effects of the present invention are as follows: compared with the prior art, a glass through-hole copper electroplating solution and copper electroplating process for radio frequency devices have the following advantages:
[0031] 1) The electroplating solution of the present invention adopts a new formula, and the composite accelerator is a compound of methylene bis(methyl)naphthalene sodium sulfonate and 5-chloro-2-methyl-4-isothiazoline-3-one, which can be adsorbed on the high potential area on the surface of the through hole, inhibit the growth of copper at the hole mouth and the surface, and is conducive to the preferential deposition of copper inside the through hole in the low potential area, thereby achieving an ideal growth mode; the wetting agent is a triblock polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F127, which is used to reduce the surface tension of the plating solution, increase the uniform distribution effect of the plating solution in the hole, and enable the metal copper to be electroplated and deposited on the seed layer of the through hole in an orderly manner.
[0032] 2) The composite leveler is a mixture of the following two components: dithienyl-pyrrolopyrrole dione: sodium carboxymethyl cellulose, which makes the copper coating crystallize finely and brightly; at the same time, it inhibits copper plating in high current density areas, and works together with other components to achieve an ideal through-hole butterfly filling mode. On the above basis, adding a trace amount of composite nucleating agents 5-nitroguaiacol sodium and 6-chloroimidazo[1,2-b]pyridazine can enhance the effects of the composite additives and strengthen the preferential nucleation filling of electroplated copper in the middle of the hole in the initial stage.
[0033] 3) In the S1 stage, using pulsed square wave current for electroplating can achieve the effect of slow surface deposition and relatively fast deposition in the hole, so that the electroplated copper is first connected in the middle of the through hole to form a butterfly wing, and then gradually deposited to the openings on both sides of the through hole, effectively avoiding the formation of holes or gaps in the through hole under other growth modes. In the S2 stage, it is adjusted to unidirectional DC output to continue filling the formed blind hole, and then complete the metallization filling of the entire through hole.
[0034] 4) By adopting a specific electroplating solution formula and adjusting the corresponding electroplating output current, rapid and void-free filling of glass through holes can be achieved in the same bath solution, while ensuring void-free metallization production and avoiding the replacement of the bath solution, thus shortening the process flow and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is an X-Ray diffraction pattern of the TGV hole obtained in the present invention after normal filling;
[0036] Figure 2 It is a cross-sectional view of butterfly filling of the TGV hole S1 stage in Example 1 of the present invention;
[0037] Figure 3 It is a cross-sectional view of the TGV hole after the S2 stage filling in Example 1 of the present invention;
[0038] Figure 4 It is a cross-sectional view of butterfly filling of the TGV hole at stage S1 in Example 2 of the present invention;
[0039] Figure 5It is a cross-sectional view of the TGV hole after the S2 stage filling in Example 2 of the present invention;
[0040] Figure 6 This is a cross-sectional view of butterfly filling of the TGV hole at stage S1 in Example 3 of the present invention;
[0041] Figure 7 It is a cross-sectional view of the TGV hole after the S2 stage filling in Example 3 of the present invention;
[0042] Figure 8 It is a cross-sectional view of butterfly filling of the TGV hole at stage S1 in the comparative example of the present invention;
[0043] Fig. 9 It is a cross-sectional view of the TGV hole after S2 stage filling in the comparative example of the present invention;
[0044] Fig.10 This is a surface image of the TGV hole after it is completely filled in the comparative example of the present invention. DETAILED DESCRIPTION
[0045] In order to more clearly describe the present invention, the present invention is further described below with reference to the accompanying drawings and text. The X-Ray diffraction pattern of the TGV hole after normal filling obtained by the present invention is Figure 1 shown.
[0046] The present invention provides a through-glass copper plating solution for radio frequency devices, comprising the following mass concentration components:
[0047] Copper methanesulfonate 250-330g / L
[0048] Methanesulfonic acid 15-35g / L
[0049] Chloride ion 40-90mg / L
[0050] Composite accelerator 120-300mg / L
[0051] Wetting agent 10-80mg / L
[0052] Composite leveling agent 20-50mg / L
[0053] Composite nucleating agent 1-8mg / L
[0054] DI pure water balance
[0055] Temperature 22-26℃
[0056] The chloride ions are provided by hydrochloric acid.
[0057] In this embodiment, the composite accelerator is sodium methylenebis(methylnaphthalene sulfonate) and 5-chloro-2-methyl-4-isothiazoline-3-one, and the mass ratio of the two when used is 5:1.
[0058] In this embodiment, the wetting agent is triblock polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F127, and its molecular formula is PEO106-PPO70-PEO106.
[0059] In this embodiment, the composite leveler is a composite of dithienyl-pyrrolopyrrole diketo and sodium carboxymethyl cellulose, and the mass concentration ratio of the two when used is 4:1.
[0060] In this embodiment, the composite nucleating agent is sodium 5-nitroguaiacol and 6-chloroimidazo[1,2-b]pyridazine, and the mass concentration ratio of the two when used is 1:1.
[0061] A copper electroplating process for through-glass vias of radio frequency devices comprises the following specific steps:
[0062] Step 1: Degrease and clean the through-hole glass plate coated with the corresponding seed layer for 5-10 minutes to remove the oil stains on the surface, and then rinse with DI pure water for 3 times to remove the excess degreaser;
[0063] Step 2: The cleaned through-hole glass plate is fixed on a double-sided electroplating apparatus and immersed in the copper electroplating solution described in any one of claims 1 to 5;
[0064] Step 3, turn on the power supply and apply S1 current, wherein the applied S1 current is a periodic commutation pulse electroplating square wave current with an off time of 10-60ms per cycle;
[0065] In step 4, a S2 current is applied, and the applied current is a unidirectional direct current.
[0066] In this embodiment, the specific conditions of step 3 are: current density 0.5-1.5ASD, plating solution circulation rate 0.5-2TO / h, electroplating time 0.5-1.0h, forward and reverse current density ratio of each cycle is 1:2-5, and forward and reverse pulse time ratio is 40-60:1.
[0067] In this embodiment, the specific conditions of step 4 are: current density of 2-5ASD, plating solution circulation rate of 3-4TO / h, and electroplating time of 1.0-2.5h.
[0068] In the S1 stage, using pulsed square wave current for electroplating can achieve the effect of slow surface deposition and relatively fast deposition in the hole, so that the electroplated copper first connects in the middle of the through hole to form butterfly wings, and then gradually deposits to the openings on both sides of the through hole, effectively avoiding the formation of holes or gaps in the through hole under other growth modes. In the S2 stage, it is adjusted to unidirectional DC output to continue filling the formed blind hole, thereby completing the metallization filling of the entire through hole.
[0069] The beneficial effects of the present invention are as follows: compared with the prior art, a glass through-hole copper electroplating solution and copper electroplating process for radio frequency devices have the following advantages:
[0070] 1) The electroplating solution of the present invention adopts a new formula, and the composite accelerator is a compound of methylene bis(methyl)naphthalene sodium sulfonate and 5-chloro-2-methyl-4-isothiazoline-3-one, which can be adsorbed on the high potential area on the surface of the through hole, inhibit the growth of copper at the hole mouth and the surface, and is conducive to the preferential deposition of copper inside the through hole in the low potential area, thereby achieving an ideal growth mode; the wetting agent is a triblock polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F127, which is used to reduce the surface tension of the plating solution, increase the uniform distribution effect of the plating solution in the hole, and enable the metal copper to be electroplated and deposited on the seed layer of the through hole in an orderly manner.
[0071] 2) The composite leveler is a mixture of the following two components: dithienyl-pyrrolopyrrole dione: sodium carboxymethyl cellulose, which makes the copper coating crystallize finely and brightly; at the same time, it inhibits copper plating in high current density areas, and works together with other components to achieve an ideal through-hole butterfly filling mode. On the above basis, adding a trace amount of composite nucleating agents 5-nitroguaiacol sodium and 6-chloroimidazo[1,2-b]pyridazine can enhance the effects of the composite additives and strengthen the preferential nucleation filling of electroplated copper in the middle of the hole in the initial stage.
[0072] 3) In the S1 stage, using pulsed square wave current for electroplating can achieve the effect of slow surface deposition and relatively fast deposition in the hole, so that the electroplated copper is first connected in the middle of the through hole to form a butterfly wing, and then gradually deposited to the openings on both sides of the through hole, effectively avoiding the formation of holes or gaps in the through hole under other growth modes. In the S2 stage, it is adjusted to unidirectional DC output to continue filling the formed blind hole, and then complete the metallization filling of the entire through hole.
[0073] 4) By adopting a specific electroplating solution formula and adjusting the corresponding electroplating output current, rapid and void-free filling of glass through holes can be achieved in the same bath solution, while ensuring void-free metallization production and avoiding the replacement of the bath solution, thus shortening the process flow and improving production efficiency.
[0074] Embodiment 1
[0075] Prepare copper electroplating solution with the following concentration components:
[0076] Copper methanesulfonate 250g / L, methanesulfonic acid 15g / L, chloride ion 40mg / L, sodium methylenebismethylnaphthalenesulfonate 100mg / L, 5-chloro-2-methyl-4-isothiazoline-3-one 20mg / L, polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F12710mg / L, dithienyl-pyrrolopyrrole dione 16mg / L, sodium carboxymethyl cellulose 4mg / L, sodium 5-nitroguaiacol 0.5mg / L, 6-chloroimidazo[1,2-b]pyridazine 0.5mg / L
[0077] DI pure water balance
[0078] Temperature 25℃
[0079] S1 electroplating conditions: apply a periodic commutation pulse electroplating square wave current with an off time of 40ms per cycle, the forward and reverse current density ratio of each cycle is 1:3, the forward and reverse pulse time ratio is 50:1, the current density is 1.0ASD, the plating solution circulation rate is 1.5TO / h, and the electroplating time is 1.0h.
[0080] S2 electroplating conditions: unidirectional DC current, current density adjusted to 3.5ASD, plating solution circulation rate 3.5TO / h, electroplating time 1.5h.
[0081] Embodiment 2
[0082] Prepare copper electroplating solution with the following concentration components:
[0083] Copper methanesulfonate 330g / L, methanesulfonic acid 35g / L, chloride ion 90mg / L, sodium methylenebismethylnaphthalenesulfonate 250mg / L, 5-chloro-2-methyl-4-isothiazoline-3-one 50mg / L, polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F12780mg / L, dithienyl-pyrrolopyrrole dione 40mg / L, sodium carboxymethyl cellulose 10mg / L, sodium 5-nitroguaiacol 4mg / L, 6-chloroimidazo[1,2-b]pyridazine 4mg / L, balance in DI pure water
[0084] Temperature 25℃
[0085] DI pure water balance
[0086] S1 electroplating conditions: apply a periodic commutation pulse electroplating square wave current with an off time of 50ms per cycle, the forward and reverse current density ratio of each cycle is 1:2, the forward and reverse pulse time ratio is 40:1, the current density is 1.5ASD, the plating solution circulation rate is 2TO / h, and the electroplating time is 1.0h.
[0087] S2 electroplating conditions: unidirectional DC current, current density adjusted to 4ASD, plating solution circulation rate 4TO / h, electroplating time 2.5h.
[0088] Embodiment 3
[0089] Prepare copper electroplating solution with the following concentration components:
[0090] Copper methanesulfonate 300g / L, methanesulfonic acid 30g / L, chloride ion 60mg / L, sodium methylenebismethylnaphthalenesulfonate 150mg / L, 5-chloro-2-methyl-4-isothiazoline-3-one 30mg / L, polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F12750mg / L, dithienyl-pyrrolopyrrole dione 20mg / L, sodium carboxymethyl cellulose 5mg / L, sodium 5-nitroguaiacol 2mg / L, 6-chloroimidazo[1,2-b]pyridazine 2mg / LDI pure water balance
[0091] Temperature 25℃
[0092] S1 electroplating conditions: apply a periodic commutation pulse electroplating square wave current with an off time of 45ms per cycle, the forward and reverse current density ratio of each cycle is 1:3, the forward and reverse pulse time ratio is 45:1, the current density is 1.5ASD, the plating solution circulation rate is 1.5TO / h, and the electroplating time is 1.0h.
[0093] S2 electroplating conditions: unidirectional DC current, current density adjusted to 3.5ASD, plating solution circulation rate 3TO / h, electroplating time 2.0h.
[0094] Comparative Example 1
[0095] Copper methanesulfonate 250g / L, methanesulfonic acid 15g / L, chloride ion 40mg / L
[0096] DI pure water balance
[0097] Temperature 25℃
[0098] S1 electroplating conditions: apply a periodic commutation pulse electroplating square wave current with an off time of 50ms per cycle, the forward and reverse current density ratio of each cycle is 1:4, the forward and reverse pulse time ratio is 60:1, the current density is 1.5ASD, the plating solution circulation rate is 0.5TO / h, and the electroplating time is 1.0h.
[0099] S2 electroplating conditions: unidirectional DC current, current density adjusted to 4.5ASD, plating solution circulation rate 3TO / h, electroplating time 2.0h.
[0100] The judging criteria are as follows:
[0101]
[0102]
[0103] Experimental groups Hole conditions Orifice Concavity Value Hole filling rate Service life Embodiment 1 excellent excellent excellent excellent Embodiment 2 excellent excellent excellent excellent Embodiment 3 excellent excellent excellent excellent Comparative Example 1 Difference Difference Difference Difference
[0104] The results obtained in Examples 1-3 are excellent, and the experimental result diagram corresponding to Example 1 is Figure 2-3 The experimental results corresponding to Example 2 are shown in 4-5, and the experimental results corresponding to Example 3 are shown in Figure 6-7 As shown, the orifice depression value is excellent, the hole filling rate is excellent, and the service life is excellent; the experimental results corresponding to the comparative example are Figure 8-10 Compared with the embodiment, it lacks composite nucleating agent, wetting agent, composite leveling agent and composite accelerator, and the result is poor, the hole mouth depression value is poor, the hole filling rate is poor, and the service life is poor.
[0105] What is disclosed are only embodiments of the present invention, but the present invention is not limited thereto, and any changes that can be conceived by those skilled in the art should fall within the protection scope of the present invention.
Claims
1. A through-glass copper plating solution for radio frequency devices, It is characterized in that The copper electroplating solution includes the following mass concentration components: Copper methanesulfonate 250-330g / L Methanesulfonic acid 15-35g / L Chloride ion 40-90mg / L Composite accelerator 120-300mg / L Wetting agent 10-80mg / L Composite leveling agent 20-50mg / L Composite nucleating agent 1-8mg / L DI pure water balance Temperature 22-26℃ The chloride ions are provided by hydrochloric acid; The composite accelerator is sodium methylenebis(methylnaphthalenesulfonate) and 5-chloro-2-methyl-4-isothiazoline-3-one, and the mass concentration ratio of the two when used is 5:1; The wetting agent is triblock polyoxyethylene-polyoxypropylene-polyoxyethylene polymer F127, whose molecular formula is PEO106-PPO70-PEO106; The composite leveler is a composite of dithienyl-pyrrolopyrrole diketo and sodium carboxymethyl cellulose, and the mass concentration ratio of the two when used is 4:1; The composite nucleating agent is sodium 5-nitroguaiacol and 6-chloroimidazo[1,2-b]pyridazine, and the mass concentration ratio of the two when used is 1:1; A copper electroplating process for the through-glass via copper electroplating solution comprises the following specific steps: Step 1: Degrease and clean the through-hole glass plate coated with the corresponding seed layer for 5-10 minutes to remove the oil stains on the surface, and then rinse with DI pure water for 3 times to remove the excess degreaser; Step 2, the cleaned through-hole glass plate is fixed on a double-sided electroplating apparatus and immersed in the electroplating copper solution; Step 3, turn on the power supply and apply S1 current, wherein the applied S1 current is a periodic commutation pulse electroplating square wave current with an off time of 10-60ms per cycle; Step 4: applying S2 current, the applied current is a unidirectional direct current; The specific conditions of step three are: current density 0.5-1.5ASD, plating solution circulation rate 0.5-2TO / h, electroplating time 0.5-1.0h, forward and reverse current density ratio of each cycle is 1:2-5, and forward and reverse pulse time ratio is 40-60:1; The specific conditions of step 4 are: current density of 2-5ASD, plating solution circulation rate of 3-4TO / h, and electroplating time of 1.0-2.5h.
Citation Information
Patent Citations
Application of acid copper leveling agent
CN103924268A
Electroplating liquid for double-sided copper plating of glass through hole and electroplating method
CN111441071A
Micro-pore electroplated copper filling method for three-dimensional (3D) copper interconnection high aspect ratio through-silicon-via technology
CN103361694A
Circuit board blind-hole hole-filling electroplating additive and preparation method thereof
CN109267118A
Blind hole-filling electroplating process, plated part obtained according to process, application of plated part, and electronic product
CN111270277A