A method for preparing carbon-fixed reinforced recycled aggregate in commercial mixing station
By mixing the waste slurry with the aggregate for carbonization treatment during the wet grinding process, a dense carbonate coating layer is formed, which solves the problems of high water absorption and high porosity of the recycled aggregate, improves its physical properties, and achieves It combines resource recovery of waste slurry and carbon sequestration of CO2, providing efficient pollution treatment and carbon emission reduction effects.
Patent Information
- Application Number
- CN202310194058.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-03
AI Technical Summary
Existing recycled aggregates have problems in application such as high water absorption, high porosity, and unsatisfactory early strength. In addition, waste slurry pollution generated during the concrete production process is difficult to effectively handle, affecting environmental protection and carbon emission reduction.
The preparation method of carbon-fixing reinforced recycled aggregates in the commercial mixing station is adopted. The waste slurry and aggregates are mixed and carbonized during the wet grinding process to form a dense carbonate coating layer, which improves the physical properties of the recycled aggregates and through The nano-calcium carbonate layer fills the interface transition zone with old cement, reducing water absorption and porosity, while using CO2 conversion to increase the carbon fixation rate.
Significantly improves the physical properties of recycled aggregates, reduces water absorption and porosity, enhances compressive strength, realizes resource recovery of waste slurry and permanent carbon sequestration of CO2, and provides efficient pollution treatment and carbon emission reduction Effect.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of comprehensive utilization of industrial solid waste carbon fixation, and in particular to a method for preparing carbon fixation-enhanced recycled aggregate for a commercial mixing station. Background Art
[0002] With the rapid development of my country's economy and the acceleration of urbanization, the construction industry has also flourished. Every year, a huge amount of waste concrete is generated due to construction and demolition. The accumulation of construction waste is one of the environmental problems that need to be solved urgently. Using construction waste to prepare recycled coarse aggregate (RCA) and applying it to concrete is one of the important measures to solve this problem, and it can effectively solve the problem of shortage of natural aggregates. However, the high water absorption rate, large crushing value and weak interface transition zone of RCA limit the large-scale application of RCA in actual engineering. In order to make the concrete prepared with recycled aggregate meet the standards of ordinary concrete, the recycled aggregate must be strengthened.
[0003] The number of mixing stations is increasing, and the requirements for green production of mixing stations are getting higher and higher. The problem of waste slurry pollution generated in the process of concrete production needs to be solved urgently. The concrete production process, concrete transportation vehicles, and site cleaning processes will produce a lot of wastewater, waste slurry, and solid waste. These waste slurries containing alkaline substances and a large amount of solid waste are directly discharged, which will seriously pollute the surrounding water resources and soil resources, and even block nearby municipal pipes, which will have a certain degree of impact on the normal life of residents. Therefore, the recycling and reuse of waste slurry and solid waste from mixing stations has received unprecedented attention. As a basic industry for economic and social development, the construction industry is closely related to carbon reduction and control, and should actively serve the realization of the "dual carbon" goals in an all-round way.
[0004] The Chinese invention patent application with application number CN202110418634.9 discloses a method for strengthening treatment of recycled aggregate, a low shrinkage mortar using recycled aggregate and a preparation method thereof. The main feature is that the recycled aggregate is strengthened by soaking it in dilute sulfuric acid and dilute acetic acid. Although the physical properties of the recycled aggregate are optimized, the strong acid and weak acid added thereto during the preparation process are costly, and the acidic substances after treatment are difficult to recover. The strong acid and weak acid remaining in the aggregate will affect the hydration of cement, causing the loss of strength of the mortar.
[0005] The Chinese invention patent application with application number CN201610833615.1 discloses a method for preparing reinforced recycled aggregate and reinforced recycled aggregate concrete, the main feature of which is to soak the recycled aggregate in a water glass and potassium methyl silicate solution for reinforcement modification. Although the recycled aggregate is modified by utilizing the unique chemical properties of the water glass and potassium methyl silicate solution, and reinforced recycled aggregate is prepared by modification, the carbon fixation rate of the aggregate is not high, the early strength is not ideal, and it is impossible to maximize carbon dioxide emission reduction. Summary of the invention
[0006] In order to actively serve the realization of the "dual carbon" goal, and at the same time solve the problems of high water absorption, high porosity, unsatisfactory early strength of recycled aggregates, and the emission pollution of solid wastes such as concrete waste slurry, the present invention provides a method for preparing carbon-fixing and strengthened recycled aggregates in a commercial mixing station. On the one hand, this method mixes waste slurry with aggregates in the wet grinding carbon fixation process to effectively improve the CO2 conversion rate. On the other hand, the alkalinity of the cement slurry on the surface of the recycled aggregate is weakened by mixed carbonization. At the same time, a new nano-calcium carbonate layer is attached to the surface of the recycled aggregate, which can be well filled and wrapped with the old cement in the interface transition zone, solving the problems of high water absorption, high porosity and low strength of the recycled aggregate itself, and preparing a new type of carbon-fixing and strengthened aggregate.
[0007] The present invention provides a method for preparing carbon-fixed reinforced recycled aggregate in a commercial mixing station, the method comprising the following steps:
[0008] Step 1: crush and separate the discarded concrete beams to obtain recycled concrete aggregate.
[0009] Step 2: Take 400-500 parts of recycled concrete aggregate, 80-100 parts of high-solid commercial waste slurry in step 1, 240-300 parts of wet grinding balls, 20-30 parts of crystal form regulators, and 180-220 parts of water, and mix them for wet grinding. During the wet grinding process, CO2 with a concentration of 40±5% and a gas rate of 2.5-3.6 kg / h is introduced into the vertical stirred mill for carbonization reaction. The reaction temperature is controlled by a water cooling device until the slurry pH is 7.3-7.6, then the CO2 is stopped, and the wet grinding is continued for 0.5h, and the wet grinding balls are removed to obtain the desired slurry.
[0010] Step 3: Put 400-750 parts of the slurry in step 2, 130-225 parts of cement, 185-295 parts of fly ash, and 20-30 parts of water into a mixer and stir at a low speed for 2-4 minutes and at a high speed for 2-4 minutes; then cast into a test block to obtain a mixed mortar. Preferably, stir at a low speed for 2 minutes and at a high speed for 2 minutes.
[0011] Step 4: Place the mixed mortar obtained in step 3 in a standard curing room with constant temperature and humidity for curing to obtain carbon-fixed reinforced recycled aggregate mortar.
[0012] Preferably, the particle size of the recycled concrete aggregate is less than 2.5 mm.
[0013] Preferably, the weight ratio of solid to water in the commercial mixed waste slurry is 0.6-0.7, and the mass value of calcium in the waste slurry accounts for 30-40%. Preferably, the weight ratio of solid to water in the commercial mixed waste slurry is 0.6.
[0014] Preferably, the wet grinding balls in step 2 are zirconia grinding bodies, and the diameter characteristics of the zirconia grinding bodies are: 0.8 mm: 0.5 mm: 0.2 mm, with a mass ratio of 2:4:4.
[0015] Preferably, in step 2, when pH=7.3-7.6, the chemical reaction equation is Ca(OH)2+CO2=CaCO3↓+H2O. If pH<7, the stable CaCO3 will continue to react with CO2 and H2O to generate soluble Ca(HCO3)2.
[0016] Preferably, the purpose of continuing wet grinding for 0.5h in step 2 is to suppress the problem of calcium carbonate volume enlargement after the carbonation reaction of the recycled aggregate and the commercial mixed waste slurry, control the particle size range of the generated nano calcium carbonate particles, and ensure that the particle size of the reinforced recycled aggregate is 0.08-5mm.
[0017] Preferably, the crystal form regulator in step 2 is potassium dihydrogen phosphate with a concentration of 5% to 10%.
[0018] Preferably, the water cooling device in step 2 is a water circulation device, and the carbonization temperature is controlled at 20±2°C by water cooling.
[0019] Preferably, in step 4, the curing temperature is 20±2° C. and the humidity is 90%.
[0020] The mechanism of the method of the present invention is as follows:
[0021] Mixing the waste aggregate and waste slurry and then subjecting them to wet grinding and carbonation treatment can separate the cement slurry attached to the surface of the waste aggregate. At the same time, the carbonized waste slurry and the residual cement slurry will form a dense carbonate coating on the surface of the aggregate, thereby optimizing the water absorption and porosity of the recycled aggregate and enhancing the physical properties of the recycled aggregate.
[0022] Waste slurry and cement paste contain alkaline ions. During the wet grinding process, the contact area between the mixed slurry and CO2 can be increased, the activity of alkaline ions can be increased, and their dissolution rate can be increased. The intense mechanical force during the wet grinding process effectively ultrafines the carbonate particles, forming a dense coating layer on the surface of the aggregate. Commercial mixed waste slurry with a solid-water weight ratio of 0.6 to 0.7 is a high-solid waste slurry. High-solid waste slurry contains more alkali metal ions. After the wet grinding carbonization reaction, it has a higher carbon fixation efficiency and is beneficial to strengthen the recycled aggregate.
[0023] The zirconia grinding body will not participate in the reaction nor be consumed during the wet grinding process, and plays a grinding role. The relevant diameter is the best ratio obtained in the test, and its grinding efficiency is the best.
[0024] Under the action of crystal modifier and temperature control, the CO2 dissolution efficiency is increased, and high-purity calcite calcium carbonate is prepared using potassium dihydrogen phosphate. In the process of preparing recycled aggregate mortar, the micro-sized carbonate microcrystals formed accelerate the cement hydration rate and fill the cracks therein, thereby improving the mortar's bending and compressive strength.
[0025] Carbonization will eliminate the incompatibility between new cement and cement attached to the surface of waste aggregates, eliminate their negative impact on the working performance of recycled aggregates, and achieve the purpose of enhancing the performance of recycled aggregates.
[0026] The present invention has the following advantages:
[0027] The wet grinding process is used to keep the calcium carbonate particles at nanometer particle size, while reducing the particle size of the recycled aggregate. The preparation process is simple, the operation is convenient, and the particle range is controllable, which is suitable for industrial large-scale production.
[0028] The mechanical force generated by wet grinding will disperse the nano calcium carbonate particles, making them evenly dispersed, allowing CO2 to fully react with calcium ions in the solution and improving carbon fixation efficiency;
[0029] The crystal form of calcium carbonate particles can be controlled by adding a small amount of potassium dihydrogen phosphate reagent during the wet grinding process. The crystal form control method is simple to operate and the crystal form is controllable.
[0030] The invention solves the conventional problems of high water absorption and high porosity of reinforced recycled aggregates. The reinforced recycled aggregates have excellent performance and can be produced on a large scale.
[0031] The prepared reinforced aggregate mortar has excellent early performance and good durability, and provides a good application approach for the CO2 mineralization of waste slurry from commercial concrete mixing plants and waste concrete. DETAILED DESCRIPTION
[0032] Example 1
[0033] (1) Take 400 parts of recycled concrete aggregate obtained by separation, mix it with 80 parts of commercial waste slurry with a water-solid ratio of 0.6 and 180 parts of water, add 20 parts of potassium dihydrogen phosphate with a concentration of 5%, 240 parts of zirconium oxide grinding bodies with a diameter of 0.8mm:0.5mm:0.2mm and a mass ratio of 2:4:4, and place the mixture in a vertical stirred mill at a speed of 700r / min and a water-cooled temperature of 20°C for 2h; during the wet grinding process, carbon dioxide gas with a concentration of 35% and a gas rate of 2.5kg / h is introduced into the vertical stirred mill for carbonization reaction. When the slurry pH is 7.3, stop introducing CO2, continue wet grinding for 0.5h, remove the wet grinding balls, and obtain slurry. The water absorption rate and apparent density are shown in Table 1.
[0034] (2) Put 480 parts of slurry, 135 parts of cement, 185 parts of fly ash and 20 parts of water in a mixer and stir at low speed for 2 minutes and at high speed for 2 minutes to obtain a mixed mortar.
[0035] (3) The mixed mortar obtained in step 2 is placed in a standard curing room with constant temperature and humidity for curing to obtain carbon-fixed reinforced recycled aggregate mortar. The 1d compressive strength, mortar water absorption rate, and chloride ion migration coefficient are shown in Table 1.
[0036] Example 2
[0037] (1) Take 450 parts of recycled concrete aggregate obtained by separation, mix it with 90 parts of commercial waste slurry with a water-solid ratio of 0.6 and 200 parts of water, add 25 parts of potassium dihydrogen phosphate with a concentration of 5%, and 270 parts of zirconium oxide grinding bodies with a diameter of 0.8mm:0.5mm:0.2mm and a mass ratio of 2:4:4, and place the mixture in a vertical stirred mill at a speed of 700r / min and water cooling to control the temperature at 20℃ for 2h; during the wet grinding process, carbon dioxide gas with a concentration of 40% and a gas rate of 2.5kg / h is introduced into the vertical stirred mill for carbonization reaction. When the slurry pH is 7.3, stop introducing CO2, continue wet grinding for 0.5h, remove the wet grinding balls, and obtain slurry. The water absorption rate and apparent density are shown in Table 1.
[0038] (2) Put 600 parts of the slurry in step 1, 175 parts of cement, 235 parts of fly ash, and 24 parts of water into a mixer and stir at low speed for 2 minutes and at high speed for 2 minutes to obtain a mixed mortar.
[0039] (3) The mixed mortar obtained in step 2 is placed in a standard curing room with constant temperature and humidity for curing to obtain carbon-fixed reinforced recycled aggregate mortar. The 1d compressive strength, mortar water absorption rate, and chloride ion migration coefficient are shown in Table 1.
[0040] Example 3
[0041] (1) Take 500 parts of recycled concrete aggregate obtained by separation, mix it with 100 parts of commercial waste slurry with a water-solid ratio of 0.6 and 220 parts of water, add 30 parts of potassium dihydrogen phosphate with a concentration of 5%, 300 parts of zirconium oxide grinding bodies with a diameter of 0.8mm:0.5mm:0.2mm and a mass ratio of 2:4:4, and place the mixture in a vertical stirred mill at a speed of 700r / min and water cooling to control the temperature at 20℃ for 2h; during the wet grinding process, carbon dioxide gas with a concentration of 45% and a gas rate of 3.6kg / h is introduced into the vertical stirred mill for carbonization reaction. When the slurry pH is 7.3, stop introducing CO2, continue wet grinding for 0.5h, remove the wet grinding balls, and obtain slurry. The water absorption rate and apparent density are shown in Table 1.
[0042] (2) Put 750 parts of the slurry in step 1, 225 parts of cement, 295 parts of fly ash, and 30 parts of water into a mixer and stir at low speed for 2 minutes and at high speed for 2 minutes to obtain a mixed mortar.
[0043] (3) The mixed mortar obtained in step 2 is placed in a standard curing room with constant temperature and humidity for curing to obtain carbon-fixed reinforced recycled aggregate mortar. The 1d compressive strength, mortar water absorption rate, and chloride ion migration coefficient are shown in Table 1.
[0044] Comparative Example 1
[0045] 400 parts of recycled concrete aggregate were spread evenly, and carbon dioxide gas with a concentration of 35% and a gas rate of 2.5 kg / h was introduced for carbonization reaction. A 1% concentration of alcohol phenolphthalein solution indicator was sprayed, and the completely carbonized sample did not turn red, and the incompletely carbonized sample turned red. The area of the carbonized sample that turned red was less than 5% by visual observation, and the reinforced recycled aggregate was obtained. 270 parts of the obtained aggregate, 135 parts of cement, 50 parts of fly ash, and 90 parts of water were put into a mixer and stirred at low speed for 2 minutes and at high speed for 2 minutes; a mixed mortar was obtained. The obtained mixed mortar was placed in a standard curing room with constant temperature and humidity for curing for 3 days to obtain a mortar test block. The water absorption rate, apparent density, 1d compressive strength, mortar water absorption rate, and chloride ion migration coefficient are shown in Table 1.
[0046] Comparative Example 2
[0047] 500 parts of recycled concrete aggregate were spread evenly, and carbon dioxide gas with a concentration of 45% and a gas velocity of 3.6 kg / h was introduced for carbonization reaction. A 1% concentration of alcohol phenolphthalein solution indicator was sprayed, and the completely carbonized sample did not turn red, and the incompletely carbonized sample turned red. The area of the carbonized sample that turned red was less than 5% by visual observation, and the reinforced recycled aggregate was obtained. 475 parts of the obtained aggregate, 225 parts of cement, 100 parts of fly ash, and 165 parts of water were put into a mixer and stirred at low speed for 2 minutes and at high speed for 2 minutes; a mixed mortar was obtained. The obtained mixed mortar was placed in a standard curing room with constant temperature and humidity for curing for 3 days to obtain a mortar test block. The water absorption rate, apparent density, 1d compressive strength, mortar water absorption rate, and chloride ion migration coefficient are shown in Table 1.
[0048] Table 1 Water absorption, apparent density, 1d compressive strength, mortar water absorption, chloride ion migration coefficient
[0049] name Water absorption Apparent density 1d compressive strength Mortar water absorption Chloride ion migration coefficient Example 1 4.35% <![CDATA[2.80kg / m 3 ]]> 9.3MPa 12.3% <![CDATA[0.9×10 -12 m 2 / s]]> Example 2 4.12% <![CDATA[2.84kg / m 3 ]]> 9.5MPa 11.8% <![CDATA[0.8×10 -12 m 2 / s]]> Example 3 3.84% <![CDATA[2.92kg / m 3 ]]> 10.2MPa 10.5% <![CDATA[0.6×10 -12 m 2 / s]]> Comparative Example 1 7.84% <![CDATA[2.34kg / m 3 ]]> 5.8MPa 15.5% <![CDATA[3.5×10 -12 m 2 / s]]> Comparative Example 2 7.72% <![CDATA[2.37kg / m 3 ]]> 6.2MPa 14.9% <![CDATA[3.8×10 -12 m 2 / s]]>
[0050] As can be seen from Table 1, the reinforced recycled aggregate obtained by carbonizing the waste concrete and commercial waste slurry using a wet grinding process can effectively improve the properties of the cement paste attached to the surface of the recycled aggregate, so that the physical properties of the recycled aggregate are enhanced. Compared with the recycled aggregate treated by ordinary carbonization, the recycled aggregate treated by the process of the present invention has a significantly reduced water absorption rate and a significantly increased apparent density. The microcalcite generated in the wet grinding carbonization process accelerates the hydration of cement and fills the pores of the attached cement paste, making the structure of the attached cement paste denser, reducing the water absorption rate of the reinforced recycled mortar, effectively increasing the compressive strength of the reinforced recycled mortar, and improving the quality of the reinforced recycled aggregate. The dense carbonate layer formed on the aggregate surface by the carbonized commercial waste slurry eliminates the incompatible properties of new and old cements, improves the interface transition zone, and thus significantly reduces the chloride ion migration coefficient.
[0051] The present invention provides a new idea for the treatment of concrete waste slurry and the strengthening of recycled aggregates. It effectively absorbs CO2 during the treatment and strengthening process to achieve the effect of permanent carbon fixation. It is green and environmentally friendly and provides a good application scenario for mineralized products. It has broad application prospects.
Claims
1. A method for preparing carbon-fixed reinforced recycled aggregate in a commercial mixing station, characterized in that: The following steps are involved: Step 1, crushing and separating the discarded concrete beams to obtain recycled concrete aggregate; Step 2: In parts by weight, 400-500 parts of recycled concrete aggregate, 80-100 parts of commercial mixed waste slurry with high solid content in step 1 are mixed with 240-300 parts of wet grinding balls, 20-30 parts of crystal form regulators, and 180-220 parts of water, and then wet-milled. During the wet-milling process, CO2 with a concentration of 40±5% and a gas velocity of 2.5-3.6 kg / h is introduced into the vertical stirred mill for carbonization reaction. The reaction temperature is controlled by a water cooling device until the slurry pH is 7.3-7.6, then the introduction of CO2 is stopped, and wet-milling is continued for 0.5 h, and the wet-milling balls are removed to obtain the desired slurry; Step 3, taking 400-750 parts of slurry, 130-225 parts of cement, 185-295 parts of fly ash and 20-30 parts of water in step 2, putting them into a mixer and stirring at low speed for 2-4 minutes and at high speed for 2-4 minutes; then pouring them into test blocks to obtain mixed mortar; Step 4, curing the mixed mortar obtained in step 3 in a standard curing room with constant temperature and humidity to obtain carbon-fixed reinforced recycled aggregate mortar; The particle size of the recycled concrete aggregate is less than 2.5 mm; The solid-water weight ratio of the commercial mixed waste slurry is 0.6, and the calcium mass value in the waste slurry accounts for 30-40%; The chemical reaction equation when pH=7.3~7.6 is Ca(OH)2+CO2=CaCO3↓+H2O. If pH<7, stable CaCO3 will continue to react with CO2 and H2O to generate soluble Ca(HCO3)2. The water cooling device in step 2 is a water circulation device, and the water cooling controls the carbonization temperature at 20±2°C; The crystal form regulator in step 2 is potassium dihydrogen phosphate with a concentration of 5% to 10%; In step 2, wet grinding is continued for 0.5 h to ensure that the particle size of the reinforced recycled aggregate is 0.08-5 mm.
2. The method for preparing carbon-fixed reinforced recycled aggregate in a commercial concrete mixing station as claimed in claim 1, characterized in that: The wet grinding balls are zirconia grinding bodies, and the diameter characteristics of the zirconia grinding bodies are: 0.8 mm: 0.5 mm: 0.2 mm, and the mass ratio is 2:4:
4.
3. A method for preparing carbon-fixed reinforced recycled aggregate in a commercial concrete mixing station as claimed in claim 1, characterized in that: In step 4, the curing temperature is 20±2° C. and the humidity is 90%.
Citation Information
Patent Citations
Preparation method of strengthened recycled aggregate and strengthened recycled aggregate concrete
CN106477929A
Reinforcement treatment method of recycled aggregate, low-self-shrinkage mortar adopting recycled aggregate, and preparation method of low-self-shrinkage mortar
CN113105171A
Mechanochemical Activation Synthesis of Calcium Potassium Hydrogen Phosphate, Calcium Potassium Phosphate, and Hydroxyapatite from Eggshells (Calcite) and Potassium Monohydrogen Phosphate
BR102019014444A2
Method for carbon dioxide strengthening of recycled concrete aggregate
CN104045251A
Recycled aggregate premixed mortar and preparation method thereof
CN109553334A