A wear-resistant and environmentally friendly highway bridge material and preparation method thereof

A composite highway bridge material with silicate and magnesium cement, reinforced with fibers and fillers, addresses temperature and moisture issues, enhancing wear resistance and durability while reducing environmental impact.

CN116283202BActive Publication Date: 2024-12-06SHENZHEN WATER CONSERVANCY & CIVIL ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310112414.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-12-06
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

Cement concrete pavements suffer from poor temperature stability, moisture absorption leading to wear and tear, and reduced service life due to magnesium cement's dehalogenation and dissolution in humid environments.

Method used

A wear-resistant and environmentally friendly highway bridge material comprising silicate cement, magnesium cement, fine sand, crushed stone, modified magnesium slag, fly ash, reinforcing fibers, and bonding fillers, with additives like N,N'-ethylene bisstearamide and a bonding filler made from polyethylene powder, hydrogel, and seaweed fiber to enhance moisture resistance and bonding strength.

Benefits of technology

Improves wear resistance and durability by preventing moisture penetration, enhancing bonding strength, and reducing carbon emissions through carbon dioxide absorption and resource utilization of magnesium slag, while maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004077288660000061
    Figure BDA0004077288660000061
  • Figure BDA0004077288660000091
    Figure BDA0004077288660000091
  • Figure BDA0004077288660000101
    Figure BDA0004077288660000101
Patent Text Reader

Abstract

The present application relates to the field of road construction materials, and specifically discloses a wear-resistant and environmentally friendly highway bridge material and a preparation method thereof. A wear-resistant and environmentally friendly highway bridge material includes the following raw materials: silicate cement, magnesium cement, mixing water, fine sand, crushed stone, modified magnesium slag, fly ash, water reducer, N, N'-ethylene bis stearamide, reinforcing fiber and bonding filler. Its preparation method is: S1, silicate cement and magnesium cement are mixed evenly to obtain mixed cement; S2, mixing mixing water and N, N'-ethylene bis stearamide are mixed evenly as liquid material; S3, after the liquid material, water reducer and mixed cement are stirred evenly, fine sand, crushed stone, modified magnesium slag and fly ash are added, and the initial mixture is stirred evenly; S4, during the stirring process of the initial mixture, reinforcing fiber and bonding filler are evenly sprinkled, and the highway bridge material is stirred evenly. The present application has the effect of improving the wear resistance and water resistance of highway bridge materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of road construction materials, and in particular to a wear-resistant and environment-friendly highway bridge material and a preparation method thereof. Background Art

[0002] At present, due to the poor temperature stability of asphalt concrete, the small temperature range between the brittle point and the softening point, and the easy formation of rutting in hot weather, the application of cement concrete pavement has become more and more extensive. However, many cement pavements will soon suffer from serious wear and tear such as peeling, pockmarking, and exposed bones after they are opened to traffic, which greatly reduces the quality of the pavement and affects the life of the pavement.

[0003] Magnesium cement is an air-hardening cementitious material obtained by mixing a magnesium chloride aqueous solution with a certain concentration and active magnesium oxide powder. Magnesium cement and a certain amount of sand and stone can be used to prepare magnesium cement highway bridge materials, overcoming the disadvantage of poor wear resistance of highway bridge materials.

[0004] However, magnesium cement easily absorbs moisture in the air, causing magnesium cement highway bridge materials to easily dehalogenate, deform or dissolve in a humid environment, resulting in reduced wear resistance of the highway bridge material pavement and shortening the service life of the highway bridge material pavement. Summary of the invention

[0005] In order to improve the water resistance and wear resistance of highway bridge materials, the present application provides a wear-resistant and environmentally friendly highway bridge material and a preparation method thereof.

[0006] In the first aspect, the present application provides a wear-resistant and environmentally friendly highway bridge material adopts the following technical solution:

[0007] A wear-resistant and environment-friendly highway bridge material comprises the following raw materials in parts by weight: 80-160 parts of silicate cement; 20-80 parts of magnesium cement; 34-72 parts of mixing water; 12-86 parts of fine sand; 10-30 parts of crushed stone; 16-30 parts of modified magnesium slag; 3-5 parts of fly ash; 1-2.6 parts of water reducing agent; 0.6-1.0 parts of N,N'-ethylene bisstearamide; 2-12 parts of reinforcing fiber; 15-25 parts of bonding filler;

[0008] The preparation steps of the bonding filler are: uniformly mixing polyethylene powder, bonding water and hydrogel as an adhesive; uniformly stirring seaweed fiber, foaming agent and part of the adhesive to obtain a mixture; drying, cutting and grinding the mixture to form a spherical core; placing the spherical core into the remaining adhesive, oscillating and stirring, drying and sieving to obtain the bonding filler.

[0009] By adopting the above technical scheme, the bonding filler is used in combination with magnesium cement and modified magnesium slag. When the highway bridge material is used, the rolling of the highway bridge pavement by vehicle tires causes the position of the material inside the highway bridge material to be deformed, the adhesive is damaged under the action of hard friction, and the seaweed fiber and the foaming agent are exposed. When rainwater penetrates into the interior of the highway bridge material, or when the highway bridge material has water droplets in it because the magnesium cement absorbs moisture in the air, the foaming agent foams in contact with water and fills the pores of the highway bridge material to prevent further penetration of moisture. At the same time, the hydrogel is cracked, and more foaming agent and seaweed fiber are exposed, thereby improving the self-compactness of the highway bridge material and thus improving the wear resistance of the highway bridge material pavement.

[0010] The exposed seaweed fiber becomes sticky under the action of sodium ion solution, which improves the bonding strength of the raw materials in the highway bridge material, thereby improving the wear resistance of the highway bridge material pavement; in addition, the seaweed fiber consumes the sodium ions in the highway bridge material, reduces the probability of alkali-aggregate reaction of the highway bridge material, and at the same time reduces the corrosion of the highway bridge material to the steel in the highway bridge, thereby improving the durability of the highway bridge.

[0011] Optionally, the blowing agent is an isocyanate-terminated prepolymer.

[0012] By adopting the above technical scheme, the carbon dioxide generated by the terminal isocyanate prepolymer when it meets water is absorbed by magnesium cement and magnesium slag, thereby reducing the carbon dioxide emission and improving the internal density of the highway bridge material, thereby improving the compressive strength and wear resistance of the highway bridge material; the terminal isocyanate prepolymer reacts with water to partially generate polyurethane urea, which on the one hand improves the adhesion of the highway bridge material, and on the other hand forms a hydrophobic film to prevent moisture in the air from penetrating into the highway bridge material, thereby reducing the probability of dissolution of magnesium cement and magnesium slag and improving the wear resistance of the road surface of the highway bridge material.

[0013] Optionally, the bonding filler further includes coarse wool fibers, and the weight ratio of the seaweed fibers to the coarse wool fibers is 2:1.

[0014] By adopting the above technical scheme, the scale layers of the coarse wool rub against each other and feel, which improves the firmness of the fixation of the seaweed fiber and the terminal isocyanate prepolymer; after the seaweed fiber becomes sticky, the flexibility of the coarse wool fiber is improved, and the bonding strength of the coarse wool fiber to the raw materials in the highway bridge material is improved, making the raw materials difficult to separate from each other, thereby improving the wear resistance of the highway bridge material.

[0015] The coarse wool fiber can be selected from dead wool. The adhesive component improves the flexibility of the dead wool. The use of dead wool improves the resource utilization rate and complies with the principle of environmental protection.

[0016] Optionally, the preparation steps of the bonding filler include: stirring seaweed fiber, terminal isocyanate prepolymer, coarse wool fiber and part of hydrogel to obtain a mixture; drying, cutting and grinding the mixture to form a spherical core; placing the spherical core into the remaining hydrogel, oscillating and stirring, drying and sieving to obtain the bonding filler.

[0017] By adopting the above technical scheme, coarse wool fibers are mixed with seaweed fibers, which increases the entanglement strength between the fibers, thereby facilitating the fixation of the terminal isocyanate prepolymer; the seaweed fibers become sticky when encountering alkaline solutions, and the alkali resistance of dead wool is better than that of fine wool fibers. Under the adhesion of sticky seaweed fibers, the coarse wool fibers play a role in entanglement and enhance adhesion, thereby improving the bonding strength between the foamed terminal isocyanate prepolymer and other raw materials in the highway bridge material, thereby improving the wear resistance of the highway bridge material pavement.

[0018] Optionally, the modified magnesium slag includes magnesium slag and a water-repellent finishing agent, and the weight ratio of the magnesium slag to the water-repellent finishing agent is 6:(1-3).

[0019] By adopting the above technical scheme, during the mixing and curing of highway bridge materials, MgO in magnesium slag absorbs moisture, and the hydrolysis products are easily lost with the moisture, resulting in internal dissolution of highway bridge materials; the water-repellent finishing agent reduces the probability of hydrolysis of magnesium slag, thereby improving the internal density of highway bridge materials, and further improving the wear resistance of highway bridge materials.

[0020] Optionally, the water-repellent finishing agent includes silicone gel and C 4 Finishing agent, the silicone gel and C 4 The weight ratio of the finishing agent is 3:2.

[0021] By adopting the above technical solution, silicone gel will C 4 The finishing agent is tightly bonded to the magnesium slag, which increases the C 4 The finishing agent has a high encapsulation rate on the magnesium slag, making it difficult for the magnesium slag to come into contact with moisture, reducing the probability of hydrolysis of the magnesium slag; the hydrophobicity of the silicone gel further improves the water repellency of the modified magnesium slag, reduces the probability of hydrolysis of the magnesium slag, and improves the internal density of the highway bridge material, thereby improving the wear resistance of the highway bridge material.

[0022] Optionally, the highway bridge material also includes 8 to 16 parts by weight of basic copper sulfate.

[0023] By adopting the above technical scheme, basic copper sulfate fixes the magnesium cement hydrolysis product MgCl 2 , reducing the probability of magnesium cement being a hydrolysis product lost with water, reducing the probability of highway bridge material dissolution, and improving the self-compactness of highway bridge materials, thereby improving the wear resistance of highway bridge materials.

[0024] In the second aspect, the present application provides a method for preparing a wear-resistant and environmentally friendly highway bridge material using the following technical solution:

[0025] A method for preparing a wear-resistant and environmentally friendly highway bridge material comprises the following steps:

[0026] S1, silicate cement and magnesium cement are evenly mixed to obtain mixed cement;

[0027] S2, mixing water and N,N'-ethylene bisstearamide uniformly as liquid material;

[0028] S3, after the liquid material, water reducing agent and mixed cement are evenly mixed, fine sand, crushed stone, modified magnesium slag and fly ash are added, and the mixture is evenly mixed to obtain a primary mixture;

[0029] S4. During the initial mixing process, the reinforcing fibers and bonding fillers are evenly sprinkled in and mixed evenly to obtain the highway bridge material.

[0030] By adopting the above technical solution, the preparation steps of highway bridge materials are simple and the product performance is stable. N,N'-ethylene bisstearamide is first mixed with mixing water to fully disperse N,N'-ethylene bisstearamide. The hydration temperature of magnesium cement is high. During the heat release process of magnesium cement hydration, N,N'-ethylene bisstearamide has wettability. After absorbing water, N,N'-ethylene bisstearamide fully exerts its dispersing and lubricating effects, thereby improving the uniformity of the dispersion of various raw materials in highway bridge materials. After cooling, it forms a colloid and adheres to other raw materials of highway bridges, thereby improving the bonding strength of various raw materials in highway bridge materials, thereby improving the wear resistance of the road surface of highway bridge materials.

[0031] In the third aspect, the present application provides a method for preparing a wear-resistant and environmentally friendly highway bridge material using the following technical solution:

[0032] A method for preparing a wear-resistant and environmentally friendly highway bridge material comprises the following steps:

[0033] S1, silicate cement and magnesium cement are evenly mixed to obtain mixed cement;

[0034] S2, mixing water and N,N'-ethylene bisstearamide uniformly as liquid material;

[0035] S3, after the liquid material, water reducing agent, basic copper sulfate and mixed cement are evenly mixed, fine sand, crushed stone, modified magnesium slag and fly ash are added, and the mixture is evenly mixed to obtain a primary mixture;

[0036] S4. During the initial mixing process, the reinforcing fibers and bonding fillers are evenly sprinkled in and mixed evenly to obtain the highway bridge material.

[0037] By adopting the above technical solution, the process steps are simple and the performance of the prepared highway bridge material is stable.

[0038] In summary, the present application includes at least one of the following beneficial technical effects:

[0039] 1. Magnesium cement absorbs carbon dioxide in the air during the hardening process, reducing carbon emissions in the environment and complying with environmental protection principles;

[0040] 2. The magnesium slag produced in the production process of magnesium metal is about 8 to 10 times the product. The treatment of magnesium slag occupies arable land. The development and utilization of magnesium slag can reduce land occupation and reduce environmental pollution, which is in line with the principle of environmental protection;

[0041] 3. The bonding filler is used in combination with magnesium cement and modified magnesium slag. When water penetrates into the interior of the highway bridge material, the foaming agent foams with water to fill the pores of the highway bridge material, preventing the water from continuing to penetrate. At the same time, the hydrogel is cracked, and more foaming agent and seaweed fiber are exposed, which improves the self-compactness of the highway bridge material, thereby improving the wear resistance of the highway bridge material pavement;

[0042] 4. The moisture in the air is absorbed by the terminal isocyanate prepolymer, which reduces the water absorption of magnesium cement, thereby reducing the probability of magnesium cement hydration, reducing the loss of magnesium cement quality and strength, and improving the wear resistance of highway bridge materials and pavement;

[0043] 5. N,N'-ethylene bis stearamide is used as a lubricant to improve the uniformity of the mixing of various raw materials in highway bridge materials. At the same time, under the action of the heat generated during the hardening process of magnesium cement, part of N,N'-ethylene bis stearamide absorbs moisture, reducing the probability of hydrolysis of magnesium cement and improving the water resistance and wear resistance of highway bridge materials;

[0044] 6. The exposed seaweed fiber becomes sticky under the action of sodium ion solution, which improves the bonding strength of the raw materials in the highway bridge material, thereby improving the wear resistance of the highway bridge material; in addition, the seaweed fiber consumes the sodium ions in the highway bridge material, reduces the probability of alkali-aggregate reaction of the highway bridge material, and at the same time reduces the corrosion of the highway bridge material to the steel during the highway bridge construction, thereby improving the durability of the highway bridge;

[0045] 7. The seaweed fiber and the terminal isocyanate prepolymer are wrapped inside the adhesive, which reduces the probability of the seaweed fiber and the terminal isocyanate prepolymer being lost during the mixing process of the highway bridge materials;

[0046] 8. Basic copper sulfate fixed magnesium cement hydrolysis product MgCl 2 , reducing the probability of magnesium cement being a hydrolysis product lost with water, reducing the probability of highway bridge material dissolution, improving the self-compactness of highway bridge materials, and thus improving the wear resistance of highway bridge material pavement;

[0047] 9. During the stirring process, the elasticity of the hydrogel provides a buffering force to the bonding filler, reducing the probability of the bonding filler breaking. DETAILED DESCRIPTION

[0048] The present application is further described in detail below in conjunction with embodiments and comparative examples.

[0049] In the following examples, if no specific conditions are specified, the reaction was carried out according to conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0050] Polycarboxylate water reducer is used as water reducer; C 4 The main chemical composition of the finishing agent is hydrocarbon, cationic water-repellent finishing agent, specific gravity 1.04 ~ 1.07g / cm 3 (25℃); water reducer is polycarboxylic acid water reducer; N,N'-ethylene bis stearamide molecular weight 593.0222, molecular formula C 38 H 76 N 2 O 2 ; The reinforcing fiber is carbon fiber with a length of 8mm, a fineness of 7μm, and a compressive strength of 100MPa; the particle size of basic copper sulfate is 800 mesh and the molecular weight is 258.1765; the molecular weight of isophorone diisocyanate is 222.28; the inhibitor is nitroxyl piperidinol TH-701; the hydroxyl value of polyester diol is 52-60mgKOH / g, and the Tg is -55℃; the hydroxyl value of hydrogenated castor oil is 178-185mgKOH / g, and the molecular weight is 938g / mol; organic bismuth C 3 0H 57 BiO 6 , density 1.145 g / mL; 2-phenoxyethyl acrylate molecular weight 192.21, LogP35.53; 2-ethoxyethyl acrylate density 1.016 g / mLat25℃.

[0051] Preparation example of modified magnesium slag

[0052] Preparation Example 1

[0053] S1, 3kg of silicone gel and 2kg of C 4 The finishing agents are mixed evenly to obtain a water-repellent finishing agent;

[0054] S2. Mix the water-repellent finishing agent with 30 kg of magnesium slag and stir evenly, and obtain modified magnesium slag after drying.

[0055] Preparation Example 2

[0056] S1, 6kg of silicone gel and 4kg of C 4 The finishing agents are mixed evenly to obtain a water-repellent finishing agent;

[0057] S2. Mix the water-repellent finishing agent with 30 kg of magnesium slag and stir evenly, and obtain modified magnesium slag after drying.

[0058] Preparation Example 3

[0059] S1, 9kg of silicone gel and 6kg of C 4 The finishing agents are mixed evenly to obtain a water-repellent finishing agent;

[0060] S2. Mix the water-repellent finishing agent with 30 kg of magnesium slag and stir evenly, and obtain modified magnesium slag after drying.

[0061] Preparation Example of Isocyanate-Terminated Prepolymer

[0062] Preparation Example 4

[0063] S1. Nitrogen was introduced into a four-necked flask to remove residual moisture, 6.58 kg of isophorone diisocyanate and 0.1 kg of polymerization inhibitor were added, and the temperature was raised to 70° C. and stirred to obtain a mixed polymer;

[0064] S2, 1.2 kg of polyester diol and 0.1 kg of hydrogenated castor oil were vacuum degassed at 120°C for 2 hours, then the mixed polymer was added and stirring was continued. 4 g of organic bismuth was added dropwise and reacted for 2 hours. Then, 1 kg of 2-phenoxyethyl acrylate and 0.4 kg of 2-ethoxyethyl acrylate were added and stirred evenly to obtain a terminal isocyanate prepolymer.

[0065] Preparation example of bonding filler

[0066] Preparation Example 5

[0067] S1. Mix 4 kg of polyethylene powder, 3 kg of bonding water and 3 kg of hydrogel evenly as an adhesive;

[0068] S2, 20 kg of seaweed fiber, 10 kg of the terminal isocyanate prepolymer prepared in Preparation Example 4 and 1 / 3 of the adhesive are stirred to obtain a mixture;

[0069] S3, drying the mixture with hot air and cutting it into blocks with a length of 15 to 20 mm, and grinding the blocks into a rounding machine to form a spherical core;

[0070] S4. Place the spherical core into the remaining adhesive, shake, stir, dry, and sieve to obtain a bonding filler with a diameter of 13 to 15 mm.

[0071] Preparation Example 6

[0072] The difference between this preparation example and preparation example 5 is that 20 kg of the terminal isocyanate prepolymer prepared in preparation example 4 is added.

[0073] Preparation Example 7

[0074] The difference between this preparation example and preparation example 5 is that 30 kg of the terminal isocyanate prepolymer prepared in preparation example 4 is added.

[0075] Preparation Example 8

[0076] The difference between this preparation example and preparation example 6 is that: S2, 20 kg of seaweed fiber, 10 kg of coarse wool fiber, 20 kg of the terminal isocyanate prepolymer prepared in preparation example 4 and 1 / 3 of the adhesive are stirred to obtain a mixture.

[0077] Preparation Example 9

[0078] The difference between this preparation example and preparation example 8 is that 20 kg of coarse wool fiber is added.

[0079] Preparation Example 10

[0080] The difference between this preparation example and preparation example 8 is that 30 kg of coarse wool fiber is added.

[0081] Preparation Example 11

[0082] The difference between this preparation example and preparation example 6 is that no seaweed fiber is added.

[0083] Preparation Example 12

[0084] The difference between this preparation example and preparation example 6 is that no terminal isocyanate prepolymer is added.

[0085] Table 1 Raw materials for Preparation Examples 5 to 12 (kg)

[0086]

[0087]

[0088] Example

[0089] Example 1

[0090] S1, 80kg of Portland cement and 20kg of magnesium cement are evenly mixed to obtain mixed cement;

[0091] S2, 34 kg of mixing water and 0.6 kg of N, N'-ethylene bisstearamide were mixed evenly as liquid material;

[0092] S3, after the liquid material of S2, 1kg of water reducing agent and the mixed cement of S1 are evenly mixed, 12kg of fine sand, 10kg of crushed stone, 16kg of modified magnesium slag prepared in Preparation Example 1 and 3kg of fly ash are added, and the mixture is evenly mixed to obtain a primary mixture;

[0093] S4. During the initial mixing process, 2 kg of reinforcing fiber and 15 kg of the bonding filler prepared in Preparation Example 5 are evenly sprinkled in, and the mixture is evenly mixed to obtain a highway bridge material.

[0094] Example 2

[0095] S1, 120kg of Portland cement and 40kg of magnesium cement are evenly mixed to obtain mixed cement;

[0096] S2, 53kg mixing water and 0.8kg N,N'-ethylene bisstearamide were mixed evenly as liquid material;

[0097] S3, after the liquid material of S2, 1.8kg of water reducing agent and the mixed cement of S1 are evenly mixed, 49kg of fine sand, 20kg of crushed stone, 23kg of modified magnesium slag prepared in Preparation Example 2 and 4kg of fly ash are added, and the mixture is evenly mixed to obtain a primary mixture;

[0098] S4. During the initial mixing process, 8 kg of reinforcing fiber and 20 kg of the bonding filler prepared in Preparation Example 6 are evenly sprinkled in, and the mixture is evenly mixed to obtain a highway bridge material.

[0099] Example 3

[0100] S1, 160kg of Portland cement and 60kg of magnesium cement are evenly mixed to obtain mixed cement;

[0101] S2, 72kg mixing water and 1kg N,N'-ethylene bisstearamide were mixed evenly as liquid material;

[0102] S3, after the liquid material of S2, 2.6kg of water reducing agent and the mixed cement of S1 are evenly mixed, 86kg of fine sand, 30kg of crushed stone, 30kg of modified magnesium slag prepared in Preparation Example 3 and 5kg of fly ash are added, and the mixture is evenly mixed to obtain a primary mixture;

[0103] S4. During the initial mixing process, 12 kg of reinforcing fiber and 25 kg of the bonding filler prepared in Preparation Example 7 are evenly sprinkled in, and the mixture is evenly mixed to obtain a highway bridge material.

[0104] Example 4

[0105] The difference between this embodiment and embodiment 2 is that 20 kg of magnesium cement is added.

[0106] Example 5

[0107] The difference between this embodiment and embodiment 2 is that 60 kg of magnesium cement is added.

[0108] Example 6

[0109] The difference between this embodiment and embodiment 2 is that 16 kg of modified magnesium slag prepared in preparation example 2 is added.

[0110] Example 7

[0111] The difference between this embodiment and embodiment 2 is that 30 kg of modified magnesium slag prepared in preparation example 2 is added.

[0112] Example 8

[0113] The difference between this embodiment and embodiment 2 is that 23 kg of modified magnesium slag prepared in preparation example 1 is added.

[0114] Example 9

[0115] The difference between this embodiment and embodiment 2 is that 23 kg of modified magnesium slag prepared in preparation example 3 is added.

[0116] Example 10

[0117] The difference between this embodiment and embodiment 2 is that 15 kg of the bonding filler prepared in preparation example 6 is added.

[0118] Embodiment 11

[0119] The difference between this embodiment and embodiment 2 is that 25 kg of the bonding filler prepared in preparation example 6 is added.

[0120] Example 12

[0121] The difference between this embodiment and embodiment 2 is that 20 kg of the bonding filler prepared in preparation example 5 is added.

[0122] Example 13 to Example 16

[0123] The difference from Example 2 is that 20 kg of the bonding fillers prepared in Preparation Examples 7 to 10 were added in sequence.

[0124] Embodiment 17

[0125] The difference between this embodiment and embodiment 2 is that: S3, after the liquid material of S2, 1kg of water reducing agent, 8kg of basic copper sulfate and the mixed cement of S1 are evenly stirred, 12kg of fine sand, 10kg of crushed stone, 16kg of modified magnesium slag prepared in preparation example 1 and 3kg of fly ash are added, and stirred evenly to obtain a primary mixture.

[0126] Embodiment 18

[0127] The difference between this embodiment and embodiment 17 is that 12 kg of basic copper sulfate is added.

[0128] Embodiment 19

[0129] The difference between this embodiment and embodiment 17 is that 16 kg of basic copper sulfate is added.

[0130] Comparative Example

[0131] Comparative Example 1

[0132] The difference between this embodiment and embodiment 2 is that magnesium cement is not added.

[0133] Comparative Example 2

[0134] The difference between this embodiment and embodiment 2 is that no modified magnesium slag is added.

[0135] Comparative Example 3

[0136] The difference between this embodiment and embodiment 2 is that the modified magnesium slag is replaced with ordinary commercially available magnesium slag.

[0137] Comparative Example 4

[0138] The difference between this embodiment and embodiment 2 is that no bonding filler is added.

[0139] Comparative Example 5

[0140] The difference between this embodiment and embodiment 2 is that 20 kg of the bonding filler of preparation example 11 is added.

[0141] Comparative Example 6

[0142] The difference between this embodiment and embodiment 2 is that 20 kg of the bonding filler of preparation example 12 is added.

[0143] Table 2 Raw materials of the embodiments and comparative examples (kg)

[0144]

[0145]

[0146] Performance testing

[0147] Test methods

[0148] 1. The compressive strength (MPa) of highway bridge materials after 28 days of curing was measured using the "6 Compressive Strength Test" method in "GBT50081-2002 Ordinary Concrete Mechanical Properties Test Standard". The test results are detailed in Table 3.

[0149] 2. The flexural strength (MPa) of highway bridge materials after 28 days of curing was measured using the “10 flexural strength test” method in “GBT50081-2002 Ordinary Concrete Mechanical Properties Test Standard”. The test results are detailed in Table 3.

[0150] 3. The test steps for carbon dioxide consumption rate are as follows:

[0151] (1) Loading highway bridge materials into prefabricated molds for casting and molding;

[0152] (2) After pouring for 24 hours, the molds were removed and the specimens were cut into 300 mm × 300 mm × 50 mm specimens. The specimens were placed in a closed space filled with automobile exhaust at a temperature of 20 ± 3°C and a relative humidity of 90% for 24 hours, and the initial and final concentrations of carbon oxides were measured.

[0153] The CO2 consumption rate is calculated as follows:

[0154]

[0155] The test results are shown in Table 3.

[0156] 4. The test steps for wear resistance loss rate are as follows

[0157] (1) Highway bridge materials are placed into prefabricated molds for casting;

[0158] (2) After 24 hours of pouring, demould and cut into two specimens of the same size. Place the two specimens in a curing room at a temperature of 20 ± 3°C and a relative humidity of 90% for 28 days;

[0159] (3) After a specimen is placed in a curing room at a temperature of 20 ± 3 °C and a relative humidity of 90% for 28 days, its standard wear resistance (MPa) is measured using the method in GB / T16925-1997 Test method for wear resistance of concrete and its products;

[0160] (4) After a specimen is placed in a curing room at a temperature of 20 ± 3°C and a relative humidity of 40% for 28 days, its dry abrasion resistance (MPa) is measured using the method in GB / T16925-1997 Test method for abrasion resistance of concrete and its products;

[0161] The calculation formula of wear resistance loss rate is as follows:

[0162]

[0163] The test results are shown in Table 3.

[0164] Table 3 Test results of various embodiments and comparative examples

[0165]

[0166] In combination with Example 1, Example 2 and Example 3 and Table 3, by adjusting the addition amount of silicate cement, magnesium cement, mixing water, fine sand, crushed stone, modified magnesium slag, fly ash, polycarboxylic acid water reducer, N,N'-ethylene bisstearamide, reinforcing fiber and bonding filler in the highway bridge material, the compressive strength, flexural strength and carbon dioxide consumption rate of the highway bridge material are improved, and the wear loss rate of the highway bridge material is reduced.

[0167] It can be seen from Example 2 and Comparative Example 1 and Table 3 that the addition of magnesium cement improves the compressive strength, flexural strength and carbon dioxide consumption rate of highway bridge materials, and improves the wear loss rate of highway bridge materials. Magnesium cement is used in combination with silicate cement. After the magnesium cement is solidified, the magnesium ions of magnesium chloride hexahydrate precipitate metal ion fillers, which improves the compressive strength and flexural strength of highway bridge materials. After the magnesium cement hardener is placed in the air, it absorbs carbon dioxide in the air to form hydrates such as magnesium carbonate, magnesium carbonate trihydrate, and basic magnesium carbonate, so that the carbon dioxide consumption rate of highway bridge materials increases. When the humidity in the environment is high, magnesium cement absorbs moisture in the air and is easily hydrolyzed, resulting in pores on the surface of highway bridge materials, reducing the internal bonding strength of highway bridge materials, and increasing the wear loss rate of highway bridge materials.

[0168] Combining Example 2, Example 4 and Example 5 and Table 3, it can be seen that with the increase in the amount of magnesium cement added, the compressive strength and flexural strength of the highway bridge material are increased and then decreased, the carbon dioxide consumption rate increases, and the wear resistance loss rate increases. The reason for the decrease in the compressive strength and flexural strength of the highway bridge material is that with the increase in the amount of magnesium cement added, the probability of the highway bridge material absorbing moisture in the air increases, and the probability of internal corrosion of the highway bridge material increases, thereby reducing the compressive strength and flexural strength of the highway bridge material and increasing the wear loss rate.

[0169] Combining Comparative Examples 2 and 3 with Table 3, it can be seen that the addition of magnesium slag improves the compressive strength, flexural strength and carbon dioxide consumption rate of highway bridge materials, but at the same time increases the wear loss rate of highway bridge materials. 2 (S) has high activity and high adhesion to highway bridge materials. The bonding strength of each raw material in the highway bridge material is improved, thereby improving the compressive strength and flexural strength of the highway bridge. In addition, magnesium slag can also absorb carbon dioxide in the air, thereby improving the carbon dioxide consumption rate of highway bridge materials. The MgO in magnesium slag absorbs moisture in the air, and the hydrolysis product magnesium chloride is easily lost with the moisture, thereby increasing the porosity inside the highway bridge material and reducing the wear resistance of the highway bridge material.

[0170] Combining Example 2 and Comparative Example 3 with Table 3, it can be seen that the magnesium slag is modified to reduce the wear resistance loss rate of highway bridge materials. The modified magnesium slag is mainly coated with a layer of water-repellent finishing agent on the surface of the magnesium slag, and the water-repellent finishing agent includes silicone gel and C 4 Finishing agent, MgO in magnesium slag absorbs water, and the hydrolysis products are easily lost with water, resulting in internal dissolution of highway bridge materials; silica gel 4 The finishing agent is tightly bonded to the magnesium slag. When the water is close to the magnesium slag, it is removed by the silicone gel.4 Finishing agent, magnesium slag is not easy to contact with water, reducing the probability of magnesium slag hydrolysis, thereby improving the internal density of highway bridge materials and reducing the wear resistance loss rate of highway bridge materials.

[0171] Combining Example 2, Example 8 and Example 9 with Table 3, it can be seen that as the amount of water-repellent finishing agent added increases, the carbon dioxide consumption rate of highway bridge materials decreases, and the wear loss first decreases and then increases. 4 The finishing agent enters the silica gel to wrap the magnesium slag, reducing the amount of carbon dioxide adsorbed by the magnesium slag and also hindering the adhesion of the magnesium slag to other particles.

[0172] Combining Example 2 and Comparative Example 4 with Table 3, it can be seen that the addition of adhesive fillers improves the compressive strength and flexural strength of highway bridge materials and reduces the loss rate of wear resistance. The adhesive filler includes adhesive, seaweed fiber and terminal isocyanate prepolymer, and the adhesive is prepared from polyethylene powder, bonding water and hydrogel. When the highway bridge material is used, the rolling of the road bridge pavement by vehicle tires causes the material position inside the highway bridge material to deform, the adhesive is damaged under the action of hard friction, the seaweed fiber and the terminal isocyanate prepolymer are exposed, the terminal isocyanate prepolymer encounters water and foams to fill the pores of the highway bridge material, preventing water from continuing to penetrate, and at the same time the hydrogel is cracked, more foaming agent and seaweed fiber are exposed, the self-compactness of the highway bridge material is improved, thereby improving the compressive strength and flexural strength of the highway bridge material, and the loss rate of wear resistance of the highway bridge material is reduced; the hydrogel improves the bonding strength of the seaweed fiber and the terminal isocyanate prepolymer, and in addition, the cement glue fixes the fluorine-containing substances released by the magnesium slag, which reduces the emission of harmful substances in the highway bridge material, which is in line with the concept of environmental protection.

[0173] In combination with Example 2, Example 10 and Example 11 and Table 3, as the amount of adhesive filler added increases, the wear resistance loss of the highway bridge material first decreases and then increases. The reason is that the strength and wear resistance of the terminal isocyanate prepolymer after foaming are lower than those of the hardened cement. As the amount of adhesive filler added increases, the overall wear resistance of the highway bridge material decreases.

[0174] In combination with Example 2 and Comparative Example 5 and Table 3, adding seaweed fiber to the bonding filler reduces the wear resistance loss rate of the highway bridge material. The exposed seaweed fiber becomes sticky under the action of the sodium ion solution, which improves the bonding strength of the raw materials in the highway bridge material, thereby improving the wear resistance of the highway bridge material.

[0175] In combination with Example 2 and Comparative Example 6 and Table 3, the end-isocyanate prepolymer is added to the bonding filler, and the wear resistance loss rate of the highway bridge material is reduced. After the end-isocyanate prepolymer is foamed, the pores in the highway bridge material are filled, and water cannot penetrate into the interior of the highway bridge material, so that the magnesium cement cannot be hydrolyzed, the probability of dissolution of the highway bridge material is reduced, and the wear resistance loss rate of the highway bridge material is reduced.

[0176] Combining Example 2, Example 12 and Example 13 with Table 3, it can be seen that as the ratio of seaweed fiber to terminal isocyanate prepolymer decreases, the compressive strength and flexural strength of the highway bridge material first increase and then decrease, and the carbon dioxide consumption rate decreases. The terminal isocyanate prepolymer generates carbon dioxide when it meets water, and the highway bridge material first absorbs the carbon dioxide generated by itself, and the carbon dioxide loss rate in the detection space decreases.

[0177] In combination with Example 2 and Example 14 and Table 3, coarse wool fiber is added to the bonding filler, and the wear resistance loss rate of the highway bridge material is reduced. The coarse wool fiber is mixed with the seaweed fiber. During the preparation of the bonding filler, the coarse wool fibers rub against each other and shrink, which improves the bonding strength of the seaweed fiber and the terminal isocyanate prepolymer, making the seaweed fiber and the terminal isocyanate prepolymer easy to be wrapped by the adhesive, and the seaweed fiber and the terminal isocyanate prepolymer are not easy to be lost when the highway bridge material is stirred and mixed. The seaweed fiber becomes sticky under the action of the alkaline solution, which facilitates the bonding of the foamed terminal isocyanate prepolymer to other raw materials of the highway bridge material, improves the self-compactness of the highway bridge material, and thus reduces the wear resistance loss rate of the highway bridge material.

[0178] In combination with Example 14, Example 15 and Example 16 and in combination with Table 3, with the increase in the amount of coarse wool fiber added, the carbon dioxide consumption of the highway bridge material first increases and then decreases. Coarse wool fiber has good air permeability, and the toughness of coarse wool fiber is enhanced under the action of sticky seaweed fiber and adhesive, and it is not easy to break. Therefore, during the use of highway bridge materials, wool fiber provides a channel for the flow of air and water vapor, which is convenient for magnesium cement and magnesium slag to absorb carbon dioxide. However, with the increase of coarse wool fiber content, the foaming rate of terminal isocyanate prepolymer increases, the carbon dioxide generated increases, the carbon dioxide consumption in the space decreases, and the carbon dioxide consumption rate of highway bridge materials decreases. In combination with Example 2 and Example 17 and in combination with Table 3, basic copper sulfate is added to the highway bridge material, the compressive strength and flexural strength of the test piece are improved, the wear resistance loss rate is reduced, and basic copper sulfate fixes the hydrolysis product of magnesium cement MgCl 2 , reducing the probability of magnesium cement being a hydrolysis product lost with water, reducing the probability of highway bridge material dissolution, and improving the self-compactness of highway bridge materials, thereby improving the compressive strength and flexural strength of highway bridge materials.

[0179] Combined with Example 17, Example 18 and Example 19 and Table 3, as the amount of basic copper sulfate added increases, the wear resistance loss of the highway bridge material first decreases and then increases. Basic copper sulfate captures free calcium oxide in the highway bridge material, and the reactant can be used as a viscosity enhancer, which improves the self-compactness of the highway bridge material, thereby improving the wear resistance of the highway bridge structure. However, magnesium cement hydrates quickly, is easy to harden, and has low later strength. As the amount of basic copper sulfate added increases, the early strength of the highway bridge material is further improved, the later strength of the highway bridge material decreases, and the wear resistance loss rate of the highway bridge material increases.

[0180] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A wear-resistant and environmentally friendly highway bridge material, characterized in that: The invention comprises the following raw materials in parts by weight: 80-160 parts of silicate cement; 20-80 parts of magnesium cement; 34-72 parts of mixing water; 12-86 parts of fine sand; 10-30 parts of crushed stone; 16-30 parts of modified magnesium slag; 3-5 parts of fly ash; and 1-2.6 parts of water reducing agent. 0.6-1.0 parts of N,N'-ethylene bisstearamide; 2-12 parts of reinforcing fiber; 15-25 parts of bonding filler; The preparation steps of the bonding filler are: mixing polyethylene powder, bonding water and hydrogel uniformly as an adhesive; stirring seaweed fiber, foaming agent and part of the adhesive uniformly to obtain a mixture; drying, cutting and grinding the mixture to form a spherical core; placing the spherical core into the remaining adhesive, shaking and stirring, drying and sieving to obtain the bonding filler; Wherein, the foaming agent is a terminal isocyanate prepolymer; The bonding filler further comprises coarse wool fiber, and the weight ratio of the seaweed fiber to the coarse wool fiber is 2:1; The modified magnesium slag comprises magnesium slag and a water-repellent finishing agent, wherein the weight ratio of the magnesium slag to the water-repellent finishing agent is 6:(1-3); The water-repellent finishing agent includes silicone gel and C4 finishing agent, and the weight ratio of the silicone gel to the C4 finishing agent is 3:

2.

2. The wear-resistant and environmentally friendly highway bridge material according to claim 1, characterized in that: The preparation steps of the bonding filler include: uniformly stirring seaweed fiber, terminal isocyanate prepolymer, coarse wool fiber and part of hydrogel to obtain a mixture; drying, cutting and grinding the mixture to form a spherical core; placing the spherical core into the remaining hydrogel, oscillating and stirring, drying and sieving to obtain the bonding filler.

3. The wear-resistant and environmentally friendly highway bridge material according to claim 1, characterized in that: The highway bridge material also includes 8 to 16 parts by weight of basic copper sulfate.

4. The method for preparing a wear-resistant and environment-friendly highway bridge material according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1, silicate cement and magnesium cement are evenly mixed to obtain mixed cement; S2, mixing water and N,N'-ethylene bisstearamide uniformly as liquid material; S3, after the liquid material, water reducing agent and mixed cement are evenly mixed, fine sand, crushed stone, modified magnesium slag and fly ash are added, and the mixture is evenly mixed to obtain a primary mixture; S4. During the initial mixing process, the reinforcing fibers and bonding fillers are evenly sprinkled in and mixed evenly to obtain the highway bridge material.

5. The method for preparing a wear-resistant and environment-friendly highway bridge material according to claim 3, characterized in that: The following steps are involved: S1, silicate cement and magnesium cement are evenly mixed to obtain mixed cement; S2, mixing water and N,N'-ethylene bisstearamide uniformly as liquid material; S3, after the liquid material, water reducing agent, basic copper sulfate and mixed cement are evenly mixed, fine sand, crushed stone, modified magnesium slag and fly ash are added, and the mixture is evenly mixed to obtain a primary mixture; S4. During the initial mixing process, the reinforcing fibers and bonding fillers are evenly sprinkled in and mixed evenly to obtain the highway bridge material.