A method for preparing Mg3Sb2 thermoelectric film

Through cosputtering and in-situ annealing technology of Mg2.5Sb2 alloy and Mg target, the limitation of wearable devices' power supply dependence on chemical batteries was solved, and a high-purity and high-performance Mg3Sb2 thermoelectric film was prepared, achieving a significant improvement in thermoelectric performance. Suitable for continuous power supply of wearable devices.

CN116288202BActive Publication Date: 2024-12-06INST OF ELECTRICAL ENG CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310183408.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-01
Publication Date
2024-12-06
Estimated Expiration
2043-03-01

AI Technical Summary

Technical Problem

The existing wearable device power supply method mainly relies on chemical batteries and requires regular charging, which limits the continuous use of the device. The research on Mg3Sb2 thermoelectric materials is mainly focused on bulk materials, and there is a lack of research on film form.

Method used

The Mg2.5Sb2 alloy target and Mg target are used as targets for DC and RF magnetron sputtering, and co-sputtering is performed on the substrate surface. The Mg3Sb2 thermoelectric film is prepared in combination with in-situ annealing technology, and the sputtering power and annealing temperature are adjusted to increase the film. purity and thermoelectric properties.

Benefits of technology

The prepared Mg3Sb2 thermoelectric film has high crystallinity, obvious interface scattering effect, greatly improved thermoelectric performance, and a power factor of 175.04uW/m/K2, which is suitable for continuous power supply of wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288202B_ABST
    Figure CN116288202B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a Mg3Sb2 thermoelectric film, and relates to the technical field of thermoelectric materials. The present invention realizes the preparation of a high-purity Mg3Sb2 thermoelectric film on a substrate by co-sputtering of direct current and radio frequency. The present invention adjusts the substrate temperature and sputtering power in the magnetron sputtering process to prepare a Mg3Sb2 film with excellent performance. The prepared film has high crystallinity and obvious interface scattering effect. Compared with bulk Mg3Sb2 material, the power factor of the prepared Mg3Sb2 thermoelectric film is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermoelectric materials, and in particular to a method for preparing a Mg3Sb2 thermoelectric film. Background Art

[0002] Wearable devices have been widely used in our lives, and power supply is an indispensable part of wearable devices. If wearable devices are to be better applied to the human body, the power supply equipment must also be as convenient as possible. Currently, almost all wearable devices on the market are powered by chemical batteries. Chemical batteries need to be charged regularly, which limits the continuous use of wearable devices to a certain extent. Thermoelectric materials are a good choice for power supply. They can use the temperature difference between the human body and the external environment to generate electricity and realize continuous power supply for wearable devices.

[0003] Thermoelectric performance is usually characterized by the dimensionless thermoelectric figure of merit ZT, where ZT = α 2 σ / κ, where α is the Seebeck coefficient, σ is the electrical conductivity, κ is the thermal conductivity, and α is the 2 σ is the power factor. Mg3Sb2 is a kind of Zintl phase hexagonal layered compound, which is a narrow-band semiconductor. At present, the research on Mg3Sb2 thermoelectric materials is mainly based on bulk materials, and there is no report on Mg3Sb2 thin films. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a Mg3Sb2 thermoelectric film with high purity and excellent thermoelectric performance.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a Mg3Sb2 thermoelectric thin film, comprising the following steps:

[0007] Mg 2.5 The Sb2 alloy target is used as the target material for DC magnetron sputtering, and the Mg target is used as the target material for RF magnetron sputtering, and DC and RF co-sputtering is performed on the substrate surface to obtain an intermediate film; the power of the DC magnetron sputtering is 80-100W; the power of the RF magnetron sputtering is 20-30W;

[0008] The intermediate film is subjected to in-situ annealing to obtain the Mg3Sb2 thermoelectric film; the in-situ annealing temperature is 550-700°C.

[0009] Preferably, the in-situ annealing time is 3 to 5 hours.

[0010] Preferably, the distance between the Mg target and the substrate is 160-200 mm.

[0011] Preferably, the Mg 2.5 The distance between the Sb2 alloy target and the substrate is 140-160 mm.

[0012] Preferably, the working gas pressure of the co-sputtering is 0.3-1Pa.

[0013] Preferably, the co-sputtering time is 20 to 40 minutes.

[0014] Preferably, the Mg 2.5 The preparation method of the Sb2 alloy target comprises:

[0015] The metal Mg and Sb are mixed in a molar ratio of Mg:Sb=2.52-2.7:2, and ball-milled to obtain a ball-milled mixture; the ball-milled mixture is hot-pressed to obtain Mg 2.5 Sb2 alloy target.

[0016] Preferably, the hot pressing pressure is 50-60 MPa, the temperature is 800-900° C., and the heat preservation and pressure holding time is 40-50 min.

[0017] Preferably, the preparation method of the Mg target comprises: ball milling metal Mg to obtain metal Mg powder; hot pressing the metal Mg powder to obtain the Mg target.

[0018] Preferably, the hot pressing pressure is 40-60 MPa, the temperature is 700-900° C., and the heat preservation and pressure holding time is 10-30 min.

[0019] The present invention provides a method for preparing a Mg3Sb2 thermoelectric film, comprising the following steps: 2.5 The Sb2 alloy target is used as the target material for DC magnetron sputtering, and the Mg target is used as the target material for RF magnetron sputtering. DC and RF co-sputtering is performed on the surface of the substrate to obtain an intermediate film; the power of the DC magnetron sputtering is 80-100W; the power of the RF magnetron sputtering is 20-30W; the intermediate film is in-situ annealed to obtain the Mg3Sb2 thermoelectric film; the temperature of the in-situ annealing is 550-700°C.

[0020] The present invention realizes the preparation of high-purity Mg3Sb2 thermoelectric thin film on a substrate by co-sputtering of direct current and radio frequency. The present invention adjusts the sputtering power and in-situ annealing temperature of the magnetron sputtering process to prepare a Mg3Sb2 thin film with excellent performance. The prepared thin film has high crystallinity and obvious interface scattering effect. Compared with bulk Mg3Sb2 material, the thermoelectric performance of the prepared Mg3Sb2 thermoelectric thin film is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1is the X-ray diffraction pattern of the thermoelectric film prepared in Comparative Example 1;

[0022] Figure 2 is the X-ray diffraction pattern of the thermoelectric film prepared in Comparative Example 2;

[0023] Figure 3 is a scanning electron microscope image of the Mg3Sb2 film prepared in Example 1;

[0024] Figure 4 This is the X-ray diffraction pattern of the Mg3Sb2 film prepared in Example 1. DETAILED DESCRIPTION

[0025] The present invention provides a method for preparing a Mg3Sb2 thermoelectric thin film, comprising the following steps:

[0026] Mg 2.5 The Sb2 alloy target is used as the target material for DC magnetron sputtering, and the Mg target is used as the target material for RF magnetron sputtering, and DC and RF co-sputtering is performed on the substrate surface to obtain an intermediate film; the power of the DC magnetron sputtering is 80-100W; the power of the RF magnetron sputtering is 20-30W;

[0027] The intermediate film is subjected to in-situ annealing to obtain the Mg3Sb2 thermoelectric film; the in-situ annealing temperature is 550-700°C.

[0028] In the present invention, the Mg 2.5 The method for preparing the Sb2 alloy target preferably comprises:

[0029] The metal Mg and Sb are mixed in a molar ratio of Mg:Sb=2.52-2.7:2, and ball-milled to obtain a ball-milled mixture; the ball-milled mixture is hot-pressed to obtain Mg 2.5 Sb2 alloy target.

[0030] In the present invention, the ball milling time is preferably 20 to 25 hours, more preferably 23 to 24 hours; the rotation speed is preferably 8000 r / min. In the present invention, the molar purity of the metal Mg and Sb is preferably above 99.999%. In the present invention, the ball milling is preferably carried out in a stainless steel ball milling tank.

[0031] In the present invention, the hot pressing pressure is preferably 50-60 MPa, more preferably 52-58 MPa, the temperature is preferably 800-900° C., more preferably 820-880° C.; the heat preservation and pressure holding time is preferably 40-50 min.

[0032] In the present invention, the method for preparing the Mg target preferably comprises: ball milling metal Mg to obtain metal Mg powder; and hot pressing the metal Mg powder to obtain the Mg target.

[0033] In the present invention, the molar purity of the metal Mg is preferably 99.999% or more. In the present invention, the ball milling time is preferably 20 to 25 hours, more preferably 23 to 24 hours; the rotation speed is preferably 8000 r / min. In the present invention, the hot pressing pressure is preferably 40 to 60 MPa, more preferably 45 to 55 MPa; the temperature is preferably 700 to 900°C, more preferably 750 to 850°C; the heat preservation and pressure holding time is preferably 10 to 30 minutes, more preferably 15 to 25 minutes.

[0034] In the present invention, the substrate is preferably a glass substrate. Before co-sputtering, the present invention preferably pre-treats the substrate; the pre-treating preferably includes: ultrasonic cleaning the substrate with alcohol and deionized water in sequence and drying. The present invention has no special requirements on the power and time of the ultrasonic cleaning, and the substrate can be cleaned. In the present invention, the drying is preferably blown with high-purity nitrogen.

[0035] The present invention uses Mg 2.5 The Sb2 alloy target is used as the target material for DC magnetron sputtering, and the Mg target is used as the target material for RF magnetron sputtering. DC and RF co-sputtering are performed on the substrate surface to obtain an intermediate film.

[0036] The present invention has no special requirements for the implementation process of the co-sputtering, and the implementation process known in the art can be used. Specifically, the present invention preferably installs two targets in the vacuum chamber of the magnetron sputtering equipment, wherein Mg 2.5 The Sb2 alloy target is connected to a DC power supply, and the Mg target is connected to an RF power supply; the substrate is mounted on the sample stage, and the vacuum chamber of the vacuum magnetron sputtering device is closed; the Mg 2.5 The distance between the Sb2 alloy target and the substrate and the distance between the Mg target and the substrate were set; the mechanical pump and the molecular pump were turned on to evacuate the vacuum to 1×10 -3 Pa; introduce 60sccm of high-purity argon gas, adjust the working gas pressure, and pre-sputter for 30 minutes; then start co-sputtering coating.

[0037] In the present invention, the Mg 2.5 The distance between the Sb2 alloy target and the substrate is preferably 140 to 160 mm, more preferably 145 to 155 mm, and further preferably 148 to 152 mm. The power of the DC magnetron sputtering is preferably 85 to 95W.

[0038] In the present invention, the distance between the Mg target and the substrate is preferably 160-200 mm, more preferably 170-190 mm, and further preferably 175-185 mm. The power of the RF magnetron sputtering is preferably 23-27W.

[0039] In the present invention, the working gas pressure of the co-sputtering is preferably 0.3-1Pa.

[0040] After obtaining the intermediate film, the present invention performs in-situ annealing on the intermediate film to obtain the Mg3Sb2 thermoelectric film.

[0041] In the present invention, the temperature of the in-situ annealing is 550-700°C, preferably 600-650°C; the time is preferably 3-5h, more preferably 3-4h. The present invention utilizes in-situ annealing to ensure that atoms are rearranged at high temperature in a vacuum environment, thereby enhancing crystallinity and purity, which is beneficial to the improvement of thermoelectric performance.

[0042] The preparation method of the Mg3Sb2 thermoelectric film provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0043] Comparative Example 1

[0044] (1) Mixing metallic Mg and Sb with a molar purity of 99.999% in a stainless steel ball mill according to a molar ratio of Mg:Sb=2.6, and ball milling. The ball milling time is 25 hours, the rotation speed is 8000r / min, and a ball milled mixture is obtained; Mixing metallic Mg with a molar purity of 99.999% in a stainless steel ball mill according to a molar ratio of Mg:Sb=2.6, and ball milling is performed. The ball milling time is 25 hours, the rotation speed is 8000r / min, and metallic Mg powder is obtained;

[0045] (2) placing the ball milled mixture in a hot pressing mold and hot pressing the mixture. The hot pressing pressure is 60 MPa, the temperature is 800° C., and the time is 45 min to obtain Mg 2.5 Sb2 alloy target. Mg powder was placed in a hot pressing mold and hot pressed at a pressure of 60 MPa, a temperature of 800°C, and a time of 30 min to obtain a Mg target.

[0046] (3) Two targets were installed in the vacuum chamber of the magnetron sputtering equipment, where Mg 2.5 The Sb2 alloy target is connected to a DC power supply, and the Mg target is connected to a radio frequency power supply.

[0047] (4) Before vacuum magnetron sputtering, the glass is pretreated, wherein the pretreatment process is as follows: placing the substrate in a beaker containing alcohol and deionized water in sequence, performing ultrasonic cleaning for 20 minutes at a power of 50 W, and then blowing the substrate dry with high-purity nitrogen to obtain a clean glass substrate;

[0048] (5) Mounting the cleaned glass substrate on the sample stage and closing the vacuum chamber of the vacuum magnetron sputtering device;

[0049] (6) Adjust Mg2.5 The distance between the Sb2 alloy target and the glass substrate is 160 mm; the distance between the Mg target and the glass substrate is adjusted to 200 mm;

[0050] (7) Turn on the mechanical pump and molecular pump in sequence to evacuate to 1×10 -3 Pa;

[0051] (8) Introduce 60 sccm of high-purity argon gas and adjust the working pressure to 1 Pa. 2.5 The power of DC magnetron sputtering of the Sb2 alloy target is 70W, and the power of RF magnetron sputtering of the Mg target is 20W, and the pre-sputtering is 30 minutes. Then the sputtering coating is started for 30 minutes to obtain a magnetron sputtering film;

[0052] (9) The thin film deposited by vacuum magnetron sputtering was further annealed in situ at an annealing temperature of 400° C. for 0.5 h.

[0053] The composition and structure of the sputtered flexible thermoelectric films were analyzed by X-ray diffractometer, forming Mg-Sb compounds with high activity, such as Figure 1 shown.

[0054] Comparative Example 2

[0055] (1) Mixing metallic Mg and Sb with a molar purity of 99.999% in a stainless steel ball mill according to a molar ratio of Mg:Sb = 2.7:2, and ball milling. The ball milling time is 25 hours, the rotation speed is 8000 r / min, and a ball milled mixture is obtained; Mixing metallic Mg with a molar purity of 99.999% in a stainless steel ball mill according to a molar ratio of Mg:Sb = 2.7:2, and ball milling is performed. The ball milling time is 25 hours, the rotation speed is 8000 r / min, and metallic Mg powder is obtained;

[0056] (2) placing the ball milled mixture in a hot pressing mold and hot pressing the mixture. The hot pressing pressure is 60 MPa, the temperature is 800° C., and the time is 45 min to obtain Mg 2.5 Sb2 alloy target. Mg powder was placed in a hot pressing mold and hot pressed at a pressure of 60 MPa, a temperature of 800°C, and a time of 30 min to obtain a Mg target.

[0057] (3) Two targets were installed in the vacuum chamber of the magnetron sputtering equipment, where Mg 2.5 The Sb2 alloy target is connected to a DC power supply, and the Mg target is connected to a radio frequency power supply.

[0058] (4) Before vacuum magnetron sputtering, the glass is pretreated. The process is as follows: the substrate is placed in a beaker containing alcohol and deionized water in turn, ultrasonically cleaned for 20 minutes at a power of 50 W, and then the substrate is blown dry with high-purity nitrogen to obtain a clean glass substrate;

[0059] (5) Mounting the cleaned glass substrate on the sample stage and closing the vacuum chamber of the vacuum magnetron sputtering device;

[0060] (6) Adjust Mg 2.5 The distance between the Sb2 alloy target and the glass substrate is 140 mm; the distance between the Mg target and the glass substrate is adjusted to 200 mm;

[0061] (7) Turn on the mechanical pump and molecular pump in sequence to evacuate to 1×10 -3 Pa;

[0062] (8) Introduce 60 sccm of high-purity argon gas and adjust the working pressure to 0.3 Pa. Mg 2.5 The power of DC magnetron sputtering of the Sb2 alloy target is 70W, and the power of RF magnetron sputtering of the Mg target is 20W, and the pre-sputtering is 30 minutes. Then the sputtering coating is started for 30 minutes to obtain a magnetron sputtering film;

[0063] (9) The thin film deposited by vacuum magnetron sputtering was further annealed in situ at an annealing temperature of 400°C and an annealing time of 5 h.

[0064] The composition and structure of the sputtered flexible thermoelectric film were analyzed by X-ray diffractometer. Compared with Example 1, the Mg3Sb2 phase was gradually formed, but there were still some impurities, such as Figure 2 shown.

[0065] Example 1

[0066] (1) Mixing metallic Mg and Sb with a molar purity of 99.999% in a stainless steel ball mill according to a molar ratio of Mg:Sb = 2.7:2, and ball milling. The ball milling time is 25 hours, the rotation speed is 8000 r / min, and a ball milled mixture is obtained; Mixing metallic Mg with a molar purity of 99.999% in a stainless steel ball mill according to a molar ratio of Mg:Sb = 2.7:2, and ball milling is performed. The ball milling time is 25 hours, the rotation speed is 8000 r / min, and metallic Mg powder is obtained;

[0067] (2) placing the ball milled mixture in a hot pressing mold and hot pressing the mixture. The hot pressing pressure is 60 MPa, the temperature is 800° C., and the time is 45 min to obtain Mg 2.5 Sb2 alloy target. Mg powder was placed in a hot pressing mold and hot pressed at a pressure of 60 MPa, a temperature of 800°C, and a time of 30 min to obtain a Mg target.

[0068] (3) Two targets were installed in the vacuum chamber of the magnetron sputtering equipment, where Mg 2.5 The Sb2 alloy target is connected to a DC power supply, and the Mg target is connected to a radio frequency power supply.

[0069] (4) Before vacuum magnetron sputtering, the glass is pretreated. The process is as follows: the substrate is placed in a beaker containing alcohol and deionized water in turn, ultrasonically cleaned for 20 minutes at a power of 50 W, and then the substrate is blown dry with high-purity nitrogen to obtain a clean glass substrate;

[0070] (5) Mounting the cleaned glass substrate on the sample stage and closing the vacuum chamber of the vacuum magnetron sputtering device;

[0071] (6) Adjust Mg 2.5 The distance between the Sb2 alloy target and the glass substrate is 140 mm; the distance between the Mg target and the glass substrate is adjusted to 200 mm;

[0072] (7) Turn on the mechanical pump and molecular pump in sequence to evacuate to 1×10 -3 Pa;

[0073] (8) Introduce 60 sccm of high-purity argon gas and adjust the working pressure to 0.3 Pa. Mg 2.5 The power of DC magnetron sputtering of the Sb2 alloy target is 90W, and the power of RF magnetron sputtering of the Mg target is 25W. The pre-sputtering is performed for 30 minutes, and then the sputtering coating is started for 30 minutes to obtain a magnetron sputtering film.

[0074] (9) The thin film deposited by vacuum magnetron sputtering was further annealed in situ at a temperature of 600°C and an annealing time of 3 h.

[0075] The surface morphology of the sample was observed by scanning electron microscopy. The surface of the Mg3Sb2 film was very smooth and dense. Figure 3 At the same time, the sputtered flexible thermoelectric film was analyzed by X-ray diffractometer, and after comparison with the standard card, it was confirmed that a high-purity Mg3Sb2 phase was formed, as shown in Figure 4 shown.

[0076] The thermoelectric performance of the Mg3Sb2 thermoelectric film prepared in Example 1 was tested, and the results are shown in Table 1.

[0077] Table 1 Thermoelectric properties of Mg3Sb2 thermoelectric films prepared in Example 1

[0078] Temperature(℃) Absolute Seebeck(uV / K) Conductivity (S / m) <![CDATA[Power factor (uW / m / K 2 )]]> 31.25 150.80 1064.87 24.22 40.83 159.94 1167.73 29.87 63.43 164.81 1417.72 38.51 85.10 160.86 1694.61 43.85 105.81 166.99 2048.02 57.11 126.39 171.87 2459.88 72.66 146.64 173.78 2929.62 88.47 167.46 185.59 3596.06 123.86 187.71 187.91 4272.26 150.86 207.98 187.83 4961.36 175.04

[0079] As shown in Table 1, the performance of Mg3Sb2 film gradually improves with the increase of temperature. When the test temperature is 207.98℃, the power factor is as high as 175.04uW / m / K 2 , indicating that it has excellent thermoelectric properties.

[0080] The thermoelectric performance of the thermoelectric films prepared in Comparative Example 1 and Comparative Example 2 was tested. The results are shown in Table 2 and Table 3.

[0081] Table 2 Thermoelectric properties of Mg3Sb2 thermoelectric films prepared in Comparative Example 1

[0082] Temperature(℃) Absolute Seebeck(uV / K) Conductivity (S / m) <![CDATA[Power factor (uW / m / K 2 )]]> 33.25 31.62 42.37 0.04 42.24 38.78 45.17 0.07 62.57 39.70 46.06 0.07 86.11 42.91 56.27 0.10 107.51 44.59 60.27 0.12 128.45 46.66 65.82 0.14 148.38 48.72 71.37 0.17 165.32 50.79 76.91 0.20 188.25 52.85 82.46 0.23 206.19 54.92 88.01 0.27

[0083] Table 3 Thermoelectric properties of Mg3Sb2 thermoelectric films prepared in Comparative Example 2

[0084] Temperature(℃) Absolute Seebeck(uV / K) Conductivity (S / m) <![CDATA[Power factor (uW / m / K 2 )]]> 30.32 30.8 30.25 0.03 40.83 35.76 33.17 0.04 59.83 41.72 39.28 0.07 86.10 46.68 48.14 0.10 104.10 50.85 58.18 0.15 122.09 54.23 69.88 0.21 141.37 59.73 83.23 0.30 160.65 66.21 102.16 0.45 179.93 69.48 121.37 0.59 199.22 71.21 140.95 0.71

[0085] Comparing Tables 2 to 3 with Table 1, it can be found that due to unreasonable settings of sputtering power and annealing temperature, Comparative Examples 1 and 2 cannot form high-purity Mg3Sb2 phase, which leads to poor thermoelectric performance of the thermoelectric film.

[0086] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a Mg3Sb2 thermoelectric thin film, characterized in that: The following steps are involved: Mg 2.5 The Sb2 alloy target is used as the target material for DC magnetron sputtering, and the Mg target is used as the target material for RF magnetron sputtering, and DC and RF co-sputtering is performed on the substrate surface to obtain an intermediate film; the power of the DC magnetron sputtering is 80-100W; the power of the RF magnetron sputtering is 20-30W; The intermediate film is subjected to in-situ annealing to obtain the Mg3Sb2 thermoelectric film; the in-situ annealing temperature is 550-700°C.

2. The preparation method according to claim 1, characterized in that: The in-situ annealing time is 3 to 5 hours.

3. The preparation method according to claim 1, characterized in that: The distance between the Mg target and the substrate is 160-200 mm.

4. The preparation method according to claim 1, characterized in that: The Mg 2.5 The distance between the Sb2 alloy target and the substrate is 140-160 mm.

5. The preparation method according to claim 1, characterized in that: The working gas pressure of the co-sputtering is 0.3-1Pa.

6. The preparation method according to claim 1, characterized in that: The co-sputtering time is 20 to 40 minutes.

7. The preparation method according to claim 1, characterized in that: The Mg 2.5 The preparation method of the Sb2 alloy target comprises: The metal Mg and Sb are mixed in a molar ratio of Mg:Sb=2.52-2.7:2, and ball-milled to obtain a ball-milled mixture; the ball-milled mixture is hot-pressed to obtain Mg 2.5 Sb2 alloy target.

8. The preparation method according to claim 7, characterized in that: The hot pressing pressure is 50-60 MPa, the temperature is 800-900° C., and the heat preservation and pressure holding time is 40-50 min.

9. The preparation method according to claim 1, characterized in that: The preparation method of the Mg target comprises: ball-milling metal Mg to obtain metal Mg powder; and hot-pressing the metal Mg powder to obtain the Mg target.

10. The preparation method according to claim 9, characterized in that: The hot pressing pressure is 40-60 MPa, the temperature is 700-900° C., and the heat preservation and pressure holding time is 10-30 minutes.

Citation Information

Patent Citations

  • Sb doped Mg2Si-based thermoelectric film and preparation method thereof

    CN105274484A

  • Method for preparing hexagonal spiral morphology bismuth telluride thermoelectric thin film

    CN106498354A

  • Method for preparing bismuth telluride thermoelectric thin film with heterostructure

    CN109554674A

  • Flexible magnesium antimonide film, preparation method and application thereof, and flexible thermoelectric device

    CN115386835A

  • Mg-sb-based thermoelement, preparation method and application thereof

    US20220020909A1