Anthraquinone hydrogenation reaction based on bimetallic ionic liquid supported catalyst

By using bimetal-ionic liquid-supported catalysts in the anthraquinone hydrogenation reaction, the existing palladium alumina catalyst has been solved, and the high efficiency of high concentration of H2O2 is achieved Production and high-quality products.

CN116354793BActive Publication Date: 2024-11-26TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111633912.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-11-26
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

The existing palladium alumina catalysts have problems such as low hydrogenation efficiency, poor stability and low dispersion in the anthraquinone hydrogenation reaction, which limits the production of high-concentration H2O2 products.

Method used

Using a bimetal-ionic liquid-supported catalyst, the metal palladium compound, additive metal compound and ionic liquid are supported on the catalyst support, and the metal nanoparticles are stabilized by the spatial limitation and electrostatic action of the ionic liquid, thereby enhancing the palladium metal nanoparticles. Dispersion and catalytic efficiency, and improve the geometric structure and electron effects of the catalyst through the second metal.

Benefits of technology

It effectively improves the quality and production efficiency of H2O2 products, enhances the stability and dispersion of palladium metal catalysts, improves hydrogenation efficiency and selectivity, and can prepare high concentrations of H2O2.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a kind of anthraquinone hydrogenation reaction based on bimetallic ionic liquid supported catalyst, comprising the following steps: step 1, placing the reduced catalyst and anthraquinone working solution in a reactor, replacing the gas in the reactor with hydrogen before the reaction, the catalyst comprising a catalyst carrier and a metal palladium compound, an auxiliary metal compound and an ionic liquid loaded on the catalyst carrier, the auxiliary metal compound being a yttrium metal compound or a zinc metal compound; step 2, raising the temperature in the reactor to be treated to the working temperature, passing H2 into the reactor to keep the pressure stable at the working pressure, and continuously stirring until the reaction is completed; step 3, adding a mixed solution of phosphoric acid and deionized water after the reaction is completed, passing oxygen to fully oxidize it, and obtaining a system containing hydrogen peroxide after extraction. By the method of the present invention, a high concentration of H2O2 can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anthraquinone hydrogenation reaction, and in particular to an anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst. Background Art

[0002] As a clean chemical product, hydrogen peroxide (H2O2) is widely used in fiber bleaching, organic synthesis and environmental protection. In recent years, with its application in the preparation of propylene oxide by propylene epoxidation and the synthesis of green caprolactam, the domestic hydrogen peroxide industry has ushered in new development opportunities. In industry, H2O2 is often prepared by the anthraquinone method, accounting for more than 95% of its total production. In this process, the catalytic hydrogenation of 2-ethylanthraquinone (2-eAQ) to produce 2-ethylhydroanthraquinone is the core step, and the commonly used catalyst is palladium alumina catalyst (Pd / Al2O3). How to improve the activation ability of the catalyst to activate the two carbonyl groups (C=O) in 2-eAQ to improve the hydrogenation efficiency and selectivity is one of the current research focuses.

[0003] The single metal Pd / Al2O3 prepared by the existing technology has the disadvantages of low dispersibility and insufficient catalytic performance. Palladium-based catalysts are the most commonly used catalysts for anthraquinone hydrogenation reactions, but there are still problems such as low hydrogenation efficiency and poor stability. Domestic and foreign scholars have improved the catalytic performance of Pd / γ-Al2O3 catalysts by adding additives (second metal or third metal), modifying carriers, and adjusting preparation methods. However, there are still problems such as large Pd metal particles, poor dispersibility, and weak interaction between active components and carriers. The above problems lead to low yields and limit the production of high-concentration H2O2 (50%) products. Summary of the invention

[0004] The purpose of the present invention is to provide an anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst in order to solve the problems existing in the production process of hydrogen peroxide products in the prior art.

[0005] The technical solution adopted to achieve the purpose of the present invention is:

[0006] An anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst comprises the following steps:

[0007] Step 1, placing a reduced catalyst and anthraquinone working solution in a reactor, replacing the gas in the reactor with hydrogen before the reaction, the catalyst comprising a catalyst carrier and a metal palladium compound, an auxiliary metal compound and an ionic liquid supported on the catalyst carrier, and the auxiliary metal compound is a yttrium metal compound or a zinc metal compound;

[0008] Step 2, raising the temperature in the reactor to the working temperature, introducing H2 into the reactor to keep the pressure stable at the working pressure, and continuously stirring until the reaction is completed;

[0009] Step 3, after the reaction is completed, a mixture of phosphoric acid and deionized water is added, oxygen is introduced to fully oxidize it, and a system containing hydrogen peroxide is obtained after extraction.

[0010] In the above technical solution, in step 2, after the temperature in the reactor rises to 60-80°C and stabilizes, the reactor speed is increased to 800-1500rpm, and H2 is introduced into the reactor to keep the pressure stable at 0.2-0.6MPa; the reaction time is 10-60min.

[0011] In the above technical solution, in step 1, the catalyst is reduced by a hydrogen-argon mixed gas, sodium borohydride, ascorbic acid, hydrazine hydrate, formaldehyde, methanol or sodium citrate, preferably, by a hydrogen-argon mixed gas.

[0012] In the above technical solution, the anthraquinone working solution in step 1 is a working solution obtained by dissolving 2-ethylanthraquinone in a mixed solvent of 1,2,4-trimethylbenzene and tri(2-ethylhexyl) phosphate.

[0013] In the above technical solution, in step 1, the concentration of 2-ethylanthraquinone in the anthraquinone working solution is 100-200 g / L.

[0014] In the above technical solution, in step 3, in the mixed solution of phosphoric acid and deionized water, the volume ratio of phosphoric acid to deionized water is (2-5):20, and the concentration of phosphoric acid is 2-8 mol / L.

[0015] In the above technical solution, the ratio of the mass fraction of the reduced catalyst in step 1 to the volume fraction of the anthraquinone working solution is (0.3-1.0): (0.03-0.12), the unit of the mass fraction is g, and the unit of the volume fraction is L.

[0016] In the above technical solution, the catalyst carrier in step 1 is a porous solid material carrier, preferably γ-Al2O3, SBA-15 molecular sieve, silicon dioxide, titanium dioxide or carbon material, more preferably, the catalyst carrier is γ-Al2O3; further, the specific surface area of ​​γ-Al2O3 is 50-500m 2 / g, pore size is 5-20nm.

[0017] In the above technical solution, the metal palladium compound is sodium tetrachloropalladate, palladium chloride, palladium acetate, palladium nitrate, palladium acetylacetonate, dichlorodiammine palladium, ammonium tetrachloropalladate or tetraamminepalladium nitrate;

[0018] In the above technical solution, the yttrium metal compound is yttrium nitrate, yttrium sulfate, yttrium carbonate or yttrium bromide, preferably yttrium nitrate;

[0019] The zinc metal compound is zinc nitrate, zinc chloride, zinc sulfate, zinc sulfide, preferably zinc nitrate.

[0020] In the above technical solution, the ionic liquid is 1-butyl-3-methylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium acetate, 1-butylsulfonic acid-3-methylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium methanesulfonate or 1-butyl-3-methylimidazolium dihydrogen phosphate.

[0021] In the above technical scheme, based on the mass of the catalyst carrier, the ratio of the loading amount of the metal palladium compound in terms of palladium, the loading amount of the auxiliary metal compound in terms of auxiliary metal, and the loading amount of the ionic liquid is (0.1-1): (0.1-1): (2-10), and the loading amount refers to the mass percentage of the substance to the carrier.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. Through the method of the present invention, a high-concentration H2O2 (50%) product can be prepared, effectively improving the quality and production efficiency of the H2O2 product.

[0024] 2. In the bimetallic-ionic liquid supported catalyst of the present invention, the size of the metal nanoparticles is limited during the formation process of the metal nanoparticles through the unique spatial confinement effect, electrostatic effect and interaction between the ionic liquid and the metal, while stabilizing the metal nanoparticles, improving the dispersion of the metal nanoparticles and reducing the occurrence of aggregation.

[0025] 3. By adding a second metal (metal zinc compound or metal Y compound), the geometric structure and electronic effect of the active components of the catalyst are improved, and the catalytic efficiency of palladium metal nanoparticles is improved. At the same time, the interaction between the ionic liquid and the catalyst carrier strengthens the interaction between the palladium nanometal and the catalyst carrier, reduces the problem of easy loss of active components during the use of the catalyst, and improves the stability of the palladium metal catalyst. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] Example 1

[0028] According to the loading amount listed in Table 1, the measured sodium chloropalladate, auxiliary metal and ionic liquid impregnation solution are dispersed and mixed to obtain an ionic liquid-bimetallic impregnation solution; the auxiliary metal is Zn or Y, and the γ-Al2O3 carrier is added to the mixed impregnation solution, stirred at 45°C for 1.5h, aged at 45°C for 3h, filtered and washed, and placed in an oven at 80°C for 12h to obtain a supported ionic liquid bimetallic catalyst.

[0029] The catalyst was reduced at a temperature of 150° C. for 4 h, a heating rate of 5° C. / min, and a 10% H2 / 90% Ar mixed gas.

[0030] The reduced catalyst was used for anthraquinone hydrogenation reaction and the activity was evaluated. The specific steps are as follows:

[0031] Step 1, placing 0.6 g of the reduced catalyst and 60 mL of anthraquinone working solution in a kettle reactor, replacing the gas in the reactor with hydrogen 5 times before the reaction, wherein the anthraquinone working solution is a 2-ethyl anthraquinone solution with a concentration of 120 g / L, and the solvent in the 2-ethyl anthraquinone solution is a mixed solvent of 1,2,4-trimethylbenzene and tri(2-ethylhexyl) phosphate;

[0032] Step 2, after the temperature in the reactor rises to 60°C and stabilizes, the speed of the reactor is increased to 1000 rpm, and H2 is introduced into the reactor to maintain a stable pressure of 0.3 MPa;

[0033] Step 3, after reacting for 15 minutes, stop stirring, open the reactor, take 2 mL of the working solution after the reaction and put it into a separatory funnel, add a mixture of 2 mL of phosphoric acid and 20 mL of deionized water into the separatory funnel, and then pass oxygen into the solution in the separatory funnel to fully oxidize it, and the concentration of the phosphoric acid is 5 mol / L;

[0034] Step 4: After oxidation for 30 minutes, extraction is performed, the aqueous layer containing hydrogen peroxide in the separatory funnel is transferred to a separatory funnel, rinsed with deionized water three times, 5 mL of sulfuric acid is added, and the amount of hydrogen peroxide in the aqueous phase is titrated with calibrated potassium permanganate, wherein the concentration of the sulfuric acid is 3 mol / L, and the concentration of the potassium permanganate is 0.0235 mol / L.

[0035] The types of promoter metals (M) and ionic liquids in the catalyst and the evaluation results of their 15-min hydrogenation efficiency are shown in Table 1 below.

[0036] Table 1 Examples 1-10 Supported ionic liquid bimetallic catalysts and their anthraquinone hydrogenation efficiency

[0037] Example Loading amount (wt%) Ionic liquid types Hydrogen efficiency (g / L) Example 1 Pd=0.3,Y=0.7,IL=4 1-Butyl-3-methylimidazole hydrogen sulfate 9.8 Example 2 Pd=0.3, Y=0.3, IL=4 1-Butyl-3-methylimidazole hydrogen sulfate 7.4 Example 3 Pd=0.3,Y=1.0,IL=4 1-Butyl-3-methylimidazole hydrogen sulfate 6.7 Example 4 Pd=0.3,Zn=0.7,IL=4 1-Butyl-3-methylimidazole hydrogen sulfate 8.0

[0038] The presence of Y increases the particle dispersion of the metal active component Pd, making the active component Pd have more surface active centers and improving the hydrogenation efficiency. In addition, Y or Zn can form a complex with the imidazolium ionic liquid, which increases the surface acidity of the carrier, is conducive to the adsorption of anthraquinone molecules, and improves the hydrogenation efficiency.

[0039] There is a geometric effect between Pd and Zn, which increases the number of isolated Pd atoms and is conducive to the uniform dispersion of Pd on the Al2O3 surface; there is electron transfer between Pd and Zn, which increases the 0 The content of the species increases the adsorption capacity of H2, which is beneficial to improving the hydrogenation efficiency.

[0040] Under this reaction condition, as shown in the following Comparative Examples 1-9, the geometric effect or electronic effect of other metals on Pd is not obvious, and the addition of auxiliary metals may mask the active sites, increasing the difficulty of combining with anthraquinone molecules, so the hydrogenation efficiency is not high.

[0041] Comparative Examples 1-9

[0042] In the same manner as in Example 1, metal Y or Zn was replaced with other metals, and the hydrogenation efficiency was evaluated, as shown in Table 2 below.

[0043] Table 2 Comparative Examples 1-9 Supported Ionic Liquid Bimetallic Catalysts and Their Anthraquinone Hydrogenation Efficiency

[0044] Comparative Example Loading amount (wt%) Auxiliary Metal M Ionic liquid types Hydrogen efficiency (g / L) Comparative Example 1 Pd=0.3,M=0.7,IL=3 La 1-Butyl-3-methylimidazolium methanesulfonate 4.8 Comparative Example 2 Pd=0.3,M=0.7,IL=4 Fe 1-Butyl-3-methylimidazole hydrogen sulfate 5.0 Comparative Example 3 Pd=0.3,M=0.7,IL=4 Mg 1-Butyl-3-methylimidazole hydrogen sulfate 6.9 Comparative Example 4 Pd=0.3,M=0.7,IL=3 Ca 1-Butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide 3.1 Comparative Example 5 Pd=0.3,M=0.7,IL=3 Co 1-Butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide 2.8 Comparative Example 6 Pd=0.3,M=0.7,IL=3 W 1-Butyl-3-methylimidazolium bromide 5.1 Comparative Example 7 Pd=0.3,M=0.7,IL=3 Mo 1-Butyl-3-methylimidazolium bromide 5.6 Comparative Example 8 Pd=0.3,M=0.7,IL=4 Li 1-Butyl-3-methylimidazole hydrogen sulfate 4.4 Comparative Example 9 Pd=0.3,M=0.7,IL=4 La 1-Butyl-3-methylimidazole hydrogen sulfate 5.8

[0045] Comparative Examples 10-14

[0046] According to the loading amount listed in Table 3, the measured sodium chloropalladate, the auxiliary metal and the ionic liquid impregnation solution are dispersed and mixed to obtain the ionic liquid-bimetallic impregnation solution; the other method steps are the same as above. The evaluation results of the catalyst 15min hydrogenation efficiency are shown in Table 3 below.

[0047] Table 3 Comparative Examples 10-14 Catalysts and Anthraquinone Hydrogenation Efficiency

[0048] Comparative Example Load Auxiliary Metal M Hydrogen efficiency (g / L) Comparative Example 10 Pd=0.3,M=0.7,IL=0 Y 3.5 Comparative Example 11 Pd=0,M=0.7,IL=0 Y 0.1 Comparative Example 12 Pd=0,M=0.7,IL=0 Zn 0.2 Comparative Example 13 Pd=0.3,M=0.7,IL=0 Zn 5.6 Comparative Example 14 Pd=0.3,M=0,IL=0 - 4.8

[0049] Comparing Comparative Examples 10-11 with Example 1, the hydrogen efficiency is significantly reduced by removing the ionic liquid or the ionic liquid and metallic palladium from the catalyst. Comparative Examples 12-13 are compared with Example 4. The hydrogen efficiency is significantly reduced by removing the ionic liquid or the ionic liquid and metallic palladium from the catalyst. It can be seen from Comparative Example 14 that the hydrogen efficiency is also significantly reduced by removing the auxiliary metal and the ionic liquid from the catalyst.

[0050] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst, characterized in that: The following steps are involved: Step 1, placing the reduced catalyst and anthraquinone working solution in a reactor, replacing the gas in the reactor with hydrogen before the reaction, the catalyst comprising a catalyst carrier and a metal palladium compound, an auxiliary metal compound and an ionic liquid supported on the catalyst carrier, the catalyst carrier being a porous solid material carrier, the auxiliary metal compound being an yttrium metal compound, and the ionic liquid being 1-butyl-3-methylimidazole hydrogen sulfate; Based on the mass of the catalyst carrier, the ratio of the loading amount of the metal palladium compound in terms of palladium, the loading amount of the auxiliary metal compound in terms of auxiliary metal, and the loading amount of the ionic liquid is 0.3:0.7:4, where the loading amount refers to the mass percentage of the substance to the carrier; Step 2: When the temperature in the reactor rises to 60-80 o After the temperature reaches 0.5 °C and stabilizes, the reactor speed is increased to 800-1500 rpm, and H2 is introduced into the reactor to maintain a stable pressure of 0.2-0.6 MPa; the reaction time is 10-60 min; Step 3, after the reaction is completed, a mixture of phosphoric acid and deionized water is added, oxygen is introduced to fully oxidize it, and a system containing hydrogen peroxide is obtained after extraction.

2. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: In the step 1, the catalyst is reduced by hydrogen-argon mixed gas, sodium borohydride, ascorbic acid, hydrazine hydrate, formaldehyde, methanol or sodium citrate.

3. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: In the step 1, the catalyst is reduced by a hydrogen-argon mixed gas.

4. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: The anthraquinone working solution in step 1 is a working solution obtained by dissolving 2-ethylanthraquinone in a mixed solvent of 1,2,4-trimethylbenzene and tri(2-ethylhexyl) phosphate.

5. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: In the step 1, the concentration of 2-ethylanthraquinone in the anthraquinone working solution is 100-200 g / L.

6. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: In step 3, in the mixed solution of phosphoric acid and deionized water, the volume ratio of phosphoric acid to deionized water is (2-5):20, and the concentration of phosphoric acid is 2-8 mol / L.

7. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: The mass fraction ratio of the reduced catalyst in step 1 to the volume fraction ratio of the anthraquinone working solution is (0.3-1.0): (0.03-0.12), the mass fraction unit is g, and the volume fraction unit is L.

8. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: The catalyst carrier in step 1 is γ-Al2O3, SBA-15 molecular sieve, silicon dioxide, titanium dioxide or carbon material.

9. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: The catalyst carrier in step 1 is γ-Al2O3, and the specific surface area of ​​γ-Al2O3 is 50-500 m 2 / g, pore size is 5-20 nm.

10. The anthraquinone hydrogenation reaction based on a bimetallic-ionic liquid supported catalyst according to claim 1, characterized in that: The metal palladium compound is sodium tetrachloropalladate, palladium chloride, palladium acetate, palladium nitrate, palladium acetylacetonate, dichlorodiamminepalladium, ammonium tetrachloropalladate or tetraamminepalladium nitrate; The yttrium metal compound is yttrium nitrate, yttrium sulfate, yttrium carbonate or yttrium bromide.