A method for preparing cobalt carbide composite photocatalyst

By heating and calcining in an oil bath in a cyanamide solution, CoC8-(SN)x nanomaterials were prepared, which solved the problems of low catalytic activity and low hydrogen production rate of cobalt carbide, and achieved high-efficiency photocatalytic hydrogen production with high product purity. And the stability is good.

CN116440939BActive Publication Date: 2024-10-15HEIHE UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310556383.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-10-15
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

The existing cobalt carbide nanomaterials have problems such as low catalytic activity, low hydrogen production rate, low product purity and difficulty in synthesis, which limit their practical application in photocatalytic hydrogen production.

Method used

A method for preparing a cobalt carbide composite photocatalyst is adopted. Cobalt nitrate hexahydrate and 2-methylimidazole are dissolved and mixed, then thioacetamide is added and reacted at a specific temperature, and then heated in an oil bath in a cyanamide solution. Finally, it is calcined under the protection of nitrogen atmosphere to generate CoC8-(SN)x nanomaterials.

Benefits of technology

This method simplifies the preparation process and improves the photocatalytic activity and hydrogen production rate of cobalt carbide. The product has high purity, and the hydrogen production is stable without obvious attenuation within 20 hours. The hydrogen production rate reaches more than 1253 micromol/g per hour.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116440939B_ABST
    Figure CN116440939B_ABST
Patent Text Reader

Abstract

A method for preparing a cobalt carbide composite photocatalyst belongs to the technical field of photocatalysts. The present invention aims to solve the problems of low catalytic activity, low hydrogen production rate, low product purity, long time and difficult synthesis of existing cobalt carbide nanomaterials. Method: 1. Prepare cobalt nitrate solution and 2-methylimidazole solution respectively; 2. Mix the cobalt nitrate solution and 2-methylimidazole solution for aging; 3. Add thioacetamide solution for reaction; 4. Immerse in cyanamide solution, heat in oil bath, and finally calcine. The present invention is used for the preparation of cobalt carbide composite photocatalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalysts. Background Art

[0002] In recent years, hydrogen energy has attracted widespread attention as a sustainable green energy source. Solar photocatalytic water splitting to produce hydrogen is an ideal method for hydrogen production. It uses inexhaustible solar energy and widely distributed water resources to produce hydrogen, and is an effective strategy to solve current energy and environmental problems. In the past few decades, a large number of photocatalysts have been widely developed and applied in photocatalytic hydrogen production. However, these photocatalysts have serious problems of poor charge transfer ability and rapid electron-hole recombination, which still faces serious inefficiency problems in the practical application of photocatalytic water splitting to produce hydrogen. Therefore, the key to the practical application of photocatalytic hydrogen production lies in the construction of photocatalysts with efficient charge transfer.

[0003] Transition metal carbides have become a very promising emerging material due to their unique electronic structure, electronic properties similar to those of precious metals, high electrical conductivity, and strong chemical stability. Transition metal carbides exhibit good catalytic performance due to orbital hybridization of carbon atoms incorporated into transition metal lattices. As a typical transition metal carbide, cobalt carbide has excellent electrical conductivity. Regarding the preparation of cobalt carbide, there are currently mainly ball milling, diffusion, impregnation and precipitation, carbon thermal reduction reaction, and synthesis gas preparation methods. However, the above methods all have disadvantages to varying degrees, such as: the ball milling method has a complex experimental procedure and low product purity; the diffusion method and carbon thermal reduction reaction method have extremely high reaction temperatures and harsh experimental conditions; the impregnation and precipitation method and synthesis gas preparation method have long experimental times and low hydrogen production rates, and cannot be used on a large scale in actual production. In addition, low catalytic activity and poor material stability are also important issues that need to be urgently addressed in the development of cobalt carbide materials. Therefore, it is of great significance and value to develop a synthesis method for cobalt carbide nanomaterials with high-efficiency photocatalytic activity. Summary of the invention

[0004] The present invention aims to solve the problems of low catalytic activity, low hydrogen production rate, low product purity, long time and difficult synthesis of existing cobalt carbide nanomaterials, and further provide a preparation method of cobalt carbide composite photocatalyst.

[0005] A method for preparing a cobalt carbide composite photocatalyst is carried out according to the following steps:

[0006] 1. Dissolving cobalt nitrate hexahydrate and 2-methylimidazole in methanol to obtain cobalt nitrate solution and 2-methylimidazole solution respectively;

[0007] 2. mixing the cobalt nitrate solution and the 2-methylimidazole solution, and then standing and aging at room temperature to obtain a reactant, washing the reactant, and then dispersing it in ethanol to obtain a mixed solution;

[0008] 3. dissolving thioacetamide in ethanol to obtain a thioacetamide solution, adding the thioacetamide solution to the mixed solution and stirring, then reacting at a temperature of 120° C. to 150° C. for 3 h to 5 h, and finally centrifuging, washing and drying to obtain cobalt sulfide nanocages;

[0009] Fourth, the cobalt sulfide nanocage is immersed in a cyanamide solution with a mass percentage of 35% to 50%, heated in an oil bath, then centrifuged, washed and dried, and finally calcined under nitrogen atmosphere to obtain CoC8-(SN) x Nanomaterials.

[0010] The beneficial effects of the present invention are:

[0011] The invention heats the cyanamide solution in an oil bath so that the cyanamide is wrapped around the inner and outer surfaces of the hollow structure of the cobalt sulfide nanocage, and reacts with the hollow cobalt sulfide during the sintering process to generate cobalt carbide and sulfur-nitrogen compounds, thereby avoiding the need for extremely high temperatures for carbon to enter the lattice of metal cobalt in other preparation methods, and the prepared cobalt carbide has excellent photocatalytic activity.

[0012] CoC8-(SN) prepared by the present invention x The photocatalytic material is a new type of CoC8 nanosheet surface loaded (SN) x Composite materials of nanoparticles, in which CoC8 nanosheets are clustered into flower-like shapes, (SN) x Nanoparticles are loaded on the surface of CoC8 nanosheets. This method is a new method for preparing high-conductivity cobalt carbide composite materials. Compared with traditional mechanical alloying and high-temperature solid phase preparation methods, this method has the characteristics of simple operation, simple experimental equipment, low requirements for preparation conditions, easy control, high purity, good experimental repeatability, uniform size of the prepared products, and greatly shortened reaction time compared with existing preparation technologies. And the CoC8-(SN) prepared by this method x The material is used as a photocatalyst in the production of hydrogen by photolysis of water. The hydrogen production rate is as high as 1253 μmol / g per hour and it exhibits long-term hydrogen production activity. The hydrogen production is stable within 20 hours without obvious attenuation.

[0013] Instruction Manual

[0014] Figure 1 CoC8-(SN) prepared in Example 1 x X-ray diffraction images of nanomaterials;

[0015] Figure 2CoC8-(SN) prepared in Example 1 x X-ray photoelectron spectroscopy of nanomaterials;

[0016] Figure 3 CoC8-(SN) prepared in Example 1 x Scanning electron microscopy images of nanomaterials;

[0017] Figure 4 CoC8-(SN) prepared in Example 2 x Scanning electron microscopy images of nanomaterials;

[0018] Figure 5 CoC8-(SN) prepared in Example 3 x Scanning electron microscopy images of nanomaterials;

[0019] Figure 6 CoC8-(SN) prepared in Example 4 x Scanning electron microscopy images and elemental imaging of nanomaterials;

[0020] Figure 7 CoC8-(SN) prepared in Example 1 x Transmission electron microscopy images of nanomaterials;

[0021] Figure 8 CoC8-(SN) prepared in Example 1 x High-resolution transmission electron microscopy images of nanomaterials;

[0022] Fig. 9 CoC8-(SN) prepared in Example 1 x Visible light absorption test curve of nanomaterials;

[0023] Fig.10 CoC8-(SN) prepared in Example 1 x Image of the nanomaterial photocatalytic water splitting and hydrogen production test after 4 cycles (each cycle is 6 hours);

[0024] Fig.11 CoC8-(SN) prepared in Example 2 x Image of the nanomaterial photocatalytic water splitting and hydrogen production test after 4 cycles (each cycle is 6 hours);

[0025] Fig.12 CoC8-(SN) prepared in Example 3 x Image of the nanomaterial photocatalytic water splitting and hydrogen production test after 4 cycles (each cycle is 6 hours);

[0026] Fig.13 CoC8-(SN) prepared in Example 4 xImage of the nanomaterial's photocatalytic water splitting and hydrogen production test after 4 cycles (each cycle is 6 hours). DETAILED DESCRIPTION

[0027] Specific implementation method 1: This implementation method is a method for preparing a cobalt carbide composite photocatalyst, which is carried out according to the following steps:

[0028] 1. Dissolving cobalt nitrate hexahydrate and 2-methylimidazole in methanol to obtain cobalt nitrate solution and 2-methylimidazole solution respectively;

[0029] 2. mixing the cobalt nitrate solution and the 2-methylimidazole solution, and then standing and aging at room temperature to obtain a reactant, washing the reactant, and then dispersing it in ethanol to obtain a mixed solution;

[0030] 3. dissolving thioacetamide in ethanol to obtain a thioacetamide solution, adding the thioacetamide solution to the mixed solution and stirring, then reacting at a temperature of 120° C. to 150° C. for 3 h to 5 h, and finally centrifuging, washing and drying to obtain cobalt sulfide nanocages;

[0031] Fourth, the cobalt sulfide nanocage is immersed in a cyanamide solution with a mass percentage of 35% to 50%, heated in an oil bath, then centrifuged, washed and dried, and finally calcined under nitrogen atmosphere to obtain CoC8-(SN) x Nanomaterials.

[0032] The beneficial effects of this embodiment are:

[0033] This embodiment uses oil bath heating in a cyanamide solution to wrap cyanamide around the inner and outer surfaces of the hollow structure of the cobalt sulfide nanocage, and reacts with the hollow cobalt sulfide during the sintering process to generate cobalt carbide and sulfur-nitrogen compounds, thereby avoiding the need for extremely high temperatures for carbon to enter the lattice of metallic cobalt in other preparation methods. The prepared cobalt carbide has excellent photocatalytic activity.

[0034] CoC8-(SN) prepared in this embodiment x The photocatalytic material is a new type of CoC8 nanosheet surface loaded (SN) x Composite materials of nanoparticles, in which CoC8 nanosheets are clustered into flower-like shapes, (SN) x Nanoparticles are loaded on the surface of CoC8 nanosheets. This method is a new method for preparing high-conductivity cobalt carbide composite materials. Compared with traditional mechanical alloying and high-temperature solid phase preparation methods, this method has the characteristics of simple operation, simple experimental equipment, low preparation conditions, easy control, high purity, good experimental repeatability, uniform product size, etc., and compared with existing preparation technologies, it greatly shortens the reaction time. And the CoC8-(SN) prepared by this method xThe material is used as a photocatalyst in the production of hydrogen by photolysis of water. The hydrogen production rate is as high as 1253 μmol / g per hour and it exhibits long-term hydrogen production activity. The hydrogen production is stable within 20 hours without obvious attenuation.

[0035] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the concentration of the cobalt nitrate solution in step 1 is 0.04 mol / L to 0.07 mol / L; the concentration of the 2-methylimidazole solution in step 1 is 0.35 mol / L to 0.50 mol / L. Others are the same as specific embodiment 1.

[0036] Specific embodiment 3: This embodiment is different from specific embodiment 1 or 2 in that the molar ratio of cobalt nitrate hexahydrate in the cobalt nitrate solution and 2-methylimidazole in the 2-methylimidazole solution in step 2 is 1:(7-9). Others are the same as specific embodiment 1 or 2.

[0037] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: in step 2, the cobalt nitrate solution and the 2-methylimidazole solution are mixed for 10 to 40 minutes at a rotation speed of 700 to 1000 r / min. The rest is the same as specific embodiments 1 to 3.

[0038] Specific implementation mode 5: This implementation mode is different from the specific implementation modes 1 to 4 in that: in step 2, the step 2 is left to stand at room temperature for 5 to 8 hours. The rest is the same as the specific implementation modes 1 to 4.

[0039] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that: in step 2, the reactants are washed with water and ethanol respectively, and then the washed reactants are dispersed in ethanol to obtain a mixed solution; the mass ratio of the washed reactants to the volume of ethanol is 1g: (20-50)mL. Others are the same as specific implementation methods 1 to 5.

[0040] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the concentration of the thioacetamide solution in step 3 is 0.21 mol / L to 0.36 mol / L; the volume ratio of the thioacetamide solution to the mixed solution in step 3 is 1:(3 to 6). Others are the same as specific embodiments 1 to 6.

[0041] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: in step three, the thioacetamide solution is added to the mixed solution, and stirred for 20 to 30 minutes at a rotation speed of 1000 r / min to 1300 r / min; the drying described in step three and step four is specifically drying for 10 to 12 hours at a temperature of 60° C. to 80° C. and under vacuum conditions. The rest is the same as specific embodiments one to seven.

[0042] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that the oil bath heating described in step 4 is specifically carried out at a temperature of 80° C. to 120° C. for 5 to 8 hours. The rest is the same as specific embodiments 1 to 8.

[0043] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that in step 4, the calcination is performed for 2h to 5h under the conditions of nitrogen atmosphere protection and sintering temperature of 450°C to 600°C. The rest is the same as specific embodiments 1 to 9.

[0044] The following examples are used to verify the beneficial effects of the present invention:

[0045] Embodiment 1:

[0046] A method for preparing a cobalt carbide composite photocatalyst is carried out according to the following steps:

[0047] 1. Dissolving cobalt nitrate hexahydrate and 2-methylimidazole in methanol to obtain cobalt nitrate solution and 2-methylimidazole solution respectively;

[0048] The concentration of the cobalt nitrate solution is 0.04 mol / L; the concentration of the 2-methylimidazole solution is 0.35 mol / L;

[0049] 2. Mixing the cobalt nitrate solution and the 2-methylimidazole solution at a rotation speed of 700 r / min for 40 min, and then standing and aging at room temperature for 5 h to obtain a reactant, washing the reactant with water and ethanol respectively, and then dispersing the washed reactant in ethanol to obtain a mixed solution;

[0050] The molar ratio of cobalt nitrate hexahydrate in the cobalt nitrate solution to 2-methylimidazole in the 2-methylimidazole solution is 4:35; the mass ratio of the reactant after washing to the volume ratio of ethanol is 1 g:20 mL;

[0051] 3. Dissolving thioacetamide in ethanol to obtain a thioacetamide solution, adding the thioacetamide solution to the mixed solution, stirring at a speed of 1000 r / min for 30 min, then reacting at a temperature of 120° C. for 5 h, and finally centrifuging, washing and drying to obtain cobalt sulfide nanocages;

[0052] The concentration of the thioacetamide solution is 0.21 mol / L; the volume ratio of the thioacetamide solution to the mixed solution is 1:3;

[0053] Fourth, the cobalt sulfide nanocage was immersed in a cyanamide solution with a mass percentage of 35%, heated in an oil bath at a temperature of 80°C for 8 hours, then centrifuged, washed and dried, and finally calcined for 5 hours under a nitrogen atmosphere at a sintering temperature of 450°C to obtain CoC8-(SN) x Nanomaterials.

[0054] The drying in step 3 and step 4 is specifically carried out at a temperature of 60° C. and under vacuum conditions for 12 hours.

[0055] Embodiment 2:

[0056] A method for preparing a cobalt carbide composite photocatalyst is carried out according to the following steps:

[0057] 1. Dissolving cobalt nitrate hexahydrate and 2-methylimidazole in methanol to obtain cobalt nitrate solution and 2-methylimidazole solution respectively;

[0058] The concentration of the cobalt nitrate solution is 0.05 mol / L; the concentration of the 2-methylimidazole solution is 0.40 mol / L;

[0059] 2. Mixing the cobalt nitrate solution and the 2-methylimidazole solution at a rotation speed of 800 r / min for 30 min, and then standing and aging at room temperature for 6 h to obtain a reactant, washing the reactant with water and ethanol respectively, and then dispersing the washed reactant in ethanol to obtain a mixed solution;

[0060] The molar ratio of cobalt nitrate hexahydrate in the cobalt nitrate solution to 2-methylimidazole in the 2-methylimidazole solution is 1:8; the mass ratio of the reactant after washing to the volume ratio of ethanol is 1g:30mL;

[0061] 3. Dissolving thioacetamide in ethanol to obtain a thioacetamide solution, adding the thioacetamide solution to the mixed solution, stirring at a rotation speed of 1100 r / min for 30 minutes, then reacting at a temperature of 130° C. for 4 hours, and finally centrifuging, washing and drying to obtain cobalt sulfide nanocages;

[0062] The concentration of the thioacetamide solution is 0.26 mol / L; the volume ratio of the thioacetamide solution to the mixed solution is 1:4;

[0063] Fourth, the cobalt sulfide nanocage was immersed in a cyanamide solution with a mass percentage of 40%, heated in an oil bath at a temperature of 90°C for 7 hours, then centrifuged, washed and dried, and finally calcined for 4 hours under a nitrogen atmosphere at a sintering temperature of 500°C to obtain CoC8-(SN) x Nanomaterials.

[0064] The drying in step 3 and step 4 is specifically carried out at a temperature of 60° C. and under vacuum conditions for 12 hours.

[0065] Embodiment three:

[0066] A method for preparing a cobalt carbide composite photocatalyst is carried out according to the following steps:

[0067] 1. Dissolving cobalt nitrate hexahydrate and 2-methylimidazole in methanol to obtain cobalt nitrate solution and 2-methylimidazole solution respectively;

[0068] The concentration of the cobalt nitrate solution is 0.06 mol / L; the concentration of the 2-methylimidazole solution is 0.45 mol / L;

[0069] 2. Mixing the cobalt nitrate solution and the 2-methylimidazole solution at a rotation speed of 900 r / min for 20 min, and then standing and aging at room temperature for 7 h to obtain a reactant, washing the reactant with water and ethanol respectively, and then dispersing the washed reactant in ethanol to obtain a mixed solution;

[0070] The molar ratio of cobalt nitrate hexahydrate in the cobalt nitrate solution to 2-methylimidazole in the 2-methylimidazole solution is 2:15; the mass ratio of the reactant after washing to the volume ratio of ethanol is 1 g:40 mL;

[0071] 3. Dissolving thioacetamide in ethanol to obtain a thioacetamide solution, adding the thioacetamide solution to the mixed solution, stirring at a speed of 1200 r / min for 20 min, then reacting at a temperature of 140° C. for 3 h, and finally centrifuging, washing and drying to obtain cobalt sulfide nanocages;

[0072] The concentration of the thioacetamide solution is 0.31 mol / L; the volume ratio of the thioacetamide solution to the mixed solution is 1:5;

[0073] Fourth, the cobalt sulfide nanocage was immersed in a cyanamide solution with a mass percentage of 45%, heated in an oil bath at a temperature of 110°C for 6 hours, then centrifuged, washed and dried, and finally calcined for 3 hours under a nitrogen atmosphere at a sintering temperature of 550°C to obtain CoC8-(SN) x Nanomaterials.

[0074] The drying in step 3 and step 4 is specifically carried out at a temperature of 60° C. and under vacuum conditions for 12 hours.

[0075] Embodiment 4:

[0076] A method for preparing a cobalt carbide composite photocatalyst is carried out according to the following steps:

[0077] 1. Dissolving cobalt nitrate hexahydrate and 2-methylimidazole in methanol to obtain cobalt nitrate solution and 2-methylimidazole solution respectively;

[0078] The concentration of the cobalt nitrate solution is 0.07 mol / L; the concentration of the 2-methylimidazole solution is 0.50 mol / L;

[0079] 2. Mixing the cobalt nitrate solution and the 2-methylimidazole solution at a rotation speed of 1000 r / min for 10 min, and then standing and aging at room temperature for 8 h to obtain a reactant, washing the reactant with water and ethanol respectively, and then dispersing the washed reactant in ethanol to obtain a mixed solution;

[0080] The molar ratio of cobalt nitrate hexahydrate in the cobalt nitrate solution to 2-methylimidazole in the 2-methylimidazole solution is 7:50; the mass ratio of the reactant after washing to the volume ratio of ethanol is 1 g:50 mL;

[0081] 3. Dissolving thioacetamide in ethanol to obtain a thioacetamide solution, adding the thioacetamide solution to the mixed solution, stirring at a speed of 1300 r / min for 20 min, then reacting at a temperature of 150° C. for 3 h, and finally centrifuging, washing and drying to obtain cobalt sulfide nanocages;

[0082] The concentration of the thioacetamide solution is 0.36 mol / L; the volume ratio of the thioacetamide solution to the mixed solution is 1:6;

[0083] Fourth, the cobalt sulfide nanocages were immersed in a cyanamide solution with a mass percentage of 50%, heated in an oil bath at a temperature of 120°C for 5 hours, then centrifuged, washed and dried, and finally calcined for 2 hours under a nitrogen atmosphere at a sintering temperature of 600°C to obtain CoC8-(SN) x Nanomaterials.

[0084] The drying in step 3 and step 4 is specifically carried out at a temperature of 60° C. and under vacuum conditions for 12 hours.

[0085] Figure 1 CoC8-(SN) prepared in Example 1 x X-ray diffraction image of nanomaterials; as can be seen from the figure, the spectrum shows CoC8 and (SN)x The characteristic peaks of X-ray diffraction show that the nanomaterial prepared in Example 1 is composed of CoC8 and (SN) x The product is composite and has no diffraction peaks of impurities, so the product has high purity.

[0086] Figure 2 CoC8-(SN) prepared in Example 1 x X-ray photoelectron spectrum of nanomaterials; As shown in the figure, CoC8-(SN) x The nanomaterial contains Co, C, S and N elements but no other elements, and the product has high purity.

[0087] Figure 3 CoC8-(SN) prepared in Example 1 x Scanning electron microscopy image of nanomaterials; the CoC8 nanosheets are 17nm to 20nm thick, clustered in a flower-like shape, and 15nm to 18nm in size (SN) x The particles are loaded in the voids of CoC8 nanosheets.

[0088] Figure 4 CoC8-(SN) prepared in Example 2 x Scanning electron microscopy image of nanomaterials; it can be seen from the figure that the thickness of CoC8 nanosheets is 13nm to 15nm, the clusters are flower-shaped, and the size is 11nm to 14nm (SN) x The particles agglomerated and loaded on the surface of CoC8 nanosheets.

[0089] Figure 5 CoC8-(SN) prepared in Example 3 x Scanning electron microscopy image of nanomaterials; it can be seen from the figure that the thickness of CoC8 nanosheets is 14nm~17nm, the clusters are flower-shaped, and the size is 13nm~17nm (SN) x The particles agglomerated and loaded on the surface of CoC8 nanosheets.

[0090] Figure 6 CoC8-(SN) prepared in Example 4 x Scanning electron microscopy images and elemental imaging of nanomaterials; it can be seen from the figure that the thickness of CoC8 nanosheets is 13nm~18nm, the clusters are flower-shaped, and the size is 10nm~12nm (SN) x The particles agglomerated and loaded on the surface of CoC8 nanosheets.

[0091] Figure 7 CoC8-(SN) prepared in Example 1 x Transmission electron microscopy image of nanomaterials; it can be seen from the figure that (SN) is loaded on the surface of the nanoflowers formed by the clusters of CoC8 nanosheets.x Nanoparticles.

[0092] Figure 8 CoC8-(SN) prepared in Example 1 x High-resolution transmission electron microscopy image of nanomaterials; it can be seen from the figure that the lattice spacing of 0.46nm corresponds to the (004) crystal plane of CoC8 nanosheets, and the lattice spacing of 0.29nm corresponds to (SN) x The (002) crystal plane of the nanoparticles further confirms that CoC8-(SN) x Formation of nanomaterials.

[0093] Fig. 9 CoC8-(SN) prepared in Example 1 x Visible light absorption test curve of nanomaterials; As can be seen from the figure, CoC8-(SN) x The maximum absorption edge of the nanomaterial is 610nm, and it has good light absorption properties in the visible light region.

[0094] CoC8-(SN) x The photocatalytic water splitting hydrogen production test of nanomaterials adopts the photocatalytic water splitting system analysis test. Before using the photocatalytic water splitting hydrogen production system for testing, it is first calibrated to make a standard curve of H2. The specific process is: different volumes of H2 are injected into the system respectively, and the corresponding function is obtained according to the relationship between the peak area of ​​different H2 detected by TCD and the injection volume of hydrogen, that is, the standard curve of H2. The amount of hydrogen evolution of the sample is tested using an online gas chromatograph (GC-7900, TCD). During the photocatalytic water splitting hydrogen production process of the sample, a 300W xenon lamp is used to vertically irradiate the reactor to 0.1gCoC8-(SN) x The nanomaterials were placed in a quartz reactor, and 80 mL of water and 20 mL of methanol were added. The peak area of ​​hydrogen was detected by TCD in real time, and the amount of hydrogen generated was calculated based on the hydrogen standard curve.

[0095] The hydrogen production rate is calculated by the following formula:

[0096]

[0097] Where: φ H2 Indicates the hydrogen evolution rate in micromoles / grams / hour; N H2 It represents the hydrogen production per unit mass of catalyst in micromoles / gram, and t represents the reaction time in hours.

[0098] Fig.10 CoC8-(SN) prepared in Example 1 x The test image of the photolysis of water to produce hydrogen by the nanomaterial after 4 cycles (each cycle is 6 hours); it can be seen from the figure that CoC8-(SN) xAs a photocatalyst used in hydrogen production by photolysis of water, the hydrogen production rate is as high as 1253 μmol / g per hour, and it exhibits long-term hydrogen production activity. The hydrogen production is stable within 20 hours without obvious attenuation.

[0099] Fig.11 CoC8-(SN) prepared in Example 2 x The test image of the photolysis of water to produce hydrogen by the nanomaterial after 4 cycles (each cycle is 6 hours); it can be seen from the figure that CoC8-(SN) x As a photocatalyst used in hydrogen production by photolysis of water, the hydrogen production rate is as high as 1430 μmol / g per hour, and it exhibits long-term hydrogen production activity. The hydrogen production is stable within 20 hours without obvious attenuation.

[0100] Fig.12 CoC8-(SN) prepared in Example 3 x The test image of the photolysis of water to produce hydrogen by the nanomaterial after 4 cycles (each cycle is 6 hours); it can be seen from the figure that CoC8-(SN) x As a photocatalyst used in hydrogen production by photolysis of water, the hydrogen production rate is as high as 1355 μmol / g per hour, and it exhibits long-term hydrogen production activity. The hydrogen production is stable within 20 hours without obvious attenuation.

[0101] Fig.13 CoC8-(SN) prepared in Example 4 x The test image of the photolysis of water to produce hydrogen by the nanomaterial after 4 cycles (each cycle is 6 hours); it can be seen from the figure that CoC8-(SN) x As a photocatalyst used in hydrogen production by photolysis of water, the hydrogen production rate is as high as 1533 μmol / g per hour, and it exhibits long-term hydrogen production activity. The hydrogen production is stable within 20 hours without obvious attenuation.

Claims

1. A method for preparing a cobalt carbide composite photocatalyst, characterized in that: It is carried out in the following steps:

1. Dissolving cobalt nitrate hexahydrate and 2-methylimidazole in methanol to obtain cobalt nitrate solution and 2-methylimidazole solution respectively; 2. mixing the cobalt nitrate solution and the 2-methylimidazole solution, and then standing and aging at room temperature to obtain a reactant, washing the reactant, and then dispersing it in ethanol to obtain a mixed solution; 3. dissolving thioacetamide in ethanol to obtain a thioacetamide solution, adding the thioacetamide solution to the mixed solution and stirring, then reacting at a temperature of 120° C. to 150° C. for 3 h to 5 h, and finally centrifuging, washing and drying to obtain cobalt sulfide nanocages; Fourth, the cobalt sulfide nanocage is immersed in a cyanamide solution with a mass percentage of 35% to 50%, heated in an oil bath, then centrifuged, washed and dried, and finally calcined under nitrogen atmosphere to obtain CoC8-(SN) x Nanomaterials.

2. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: The concentration of the cobalt nitrate solution described in step 1 is 0.04 mol / L to 0.07 mol / L; the concentration of the 2-methylimidazole solution described in step 1 is 0.35 mol / L to 0.50 mol / L.

3. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: The molar ratio of cobalt nitrate hexahydrate in the cobalt nitrate solution in step 2 to 2-methylimidazole in the 2-methylimidazole solution is 1:(7-9).

4. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: In step 2, the cobalt nitrate solution and the 2-methylimidazole solution are mixed at a rotation speed of 700 r / min to 1000 r / min for 10 min to 40 min.

5. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: In step 2, the mixture is allowed to stand at room temperature for 5 to 8 hours.

6. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: In step 2, the reactants are washed with water and ethanol respectively, and then the washed reactants are dispersed in ethanol to obtain a mixed solution; the mass ratio of the washed reactants to the volume of ethanol is 1g:(20-50)mL.

7. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: The concentration of the thioacetamide solution in step 3 is 0.21 mol / L to 0.36 mol / L; the volume ratio of the thioacetamide solution in step 3 to the mixed solution is 1:(3 to 6).

8. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: In step 3, the thioacetamide solution is added to the mixed solution, and stirred for 20 min to 30 min at a rotation speed of 1000 r / min to 1300 r / min; the drying described in step 3 and step 4 is specifically drying for 10 h to 12 h at a temperature of 60° C. to 80° C. and under vacuum conditions.

9. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: The oil bath heating described in step 4 is specifically heating in the oil bath at a temperature of 80° C. to 120° C. for 5 h to 8 h.

10. The method for preparing a cobalt carbide composite photocatalyst according to claim 1, characterized in that: In step 4, calcination is performed for 2 h to 5 h under the condition of nitrogen atmosphere protection and sintering temperature of 450° C. to 600° C.

Citation Information

Patent Citations

  • Cobalt sulfide / nitrogen-sulfur-codoped carbon hollow sphere composite material and preparation method thereof

    CN105140535A

  • Preparation method of cage-shaped cobalt sulfide / graphite-phase carbon nitride composite photocatalyst

    CN110586160A

  • Preparation method of in-situ defect modified Co9S8-porous nitrogen-doped carbon electrode

    CN110690469A

  • Nitrogen-doped carbon layer coated cobalt manganese carbide composite material and application thereof

    CN111617790A

  • Preparation method and application of bifunctional catalyst for high-selectivity preparation of isobutyraldehyde by propylene hydroformylation

    CN112169829A