Production process of high-purity silver nitrate, high-purity silver nitrate and its application

Through the multi-step demulsification process of adsorption-ion exchange and chelating resin, combined with high-speed centrifugal equipment and pH adjustment crystallization process, the problem of incomplete removal of impurity ions in the existing silver nitrate process is solved, and the silver nitrate is significantly improved Purity provides high-purity materials for solar cells and promotes the development of the industrial chain.

CN116462221BActive Publication Date: 2024-11-08DAGAO IND TECH RES INST (GUANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310304737.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-11-08
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

The existing silver nitrate preparation process has poor selectivity for metal ions, which makes it difficult to completely remove impurity ions, affecting the quality of silver nitrate products.

Method used

Using the combination technology of adsorption-ion exchange dual-function resin and chelating resin, combined with high-speed tube centrifugal equipment, multiple impurity removal and filtration are carried out to gradually improve the purity of silver nitrate, and finally the crystallization process is carried out by adjusting the pH value to obtain high purity. Silver nitrate.

Benefits of technology

It has achieved efficient and thorough removal of impurity ions such as Cu, Ni, Fe, Cr, etc., significantly improved the purity of silver nitrate, and the impurity content is much lower than that of conventional methods. It is suitable for high efficiency and high life solar cell silver powder materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116462221B_ABST
    Figure CN116462221B_ABST
Patent Text Reader

Abstract

The present invention provides a production process of high-purity silver nitrate, high-purity silver nitrate and its application, and specifically relates to the field of solar cell technology. The production process first reacts silver ingots with concentrated nitric acid to obtain a crude silver nitrate solution with a pH value of ≥3; then adds an adsorption-ion exchange bifunctional resin to the crude silver nitrate solution for a first impurity removal and filters to obtain a first silver nitrate solution; continues to add a chelating resin for a second impurity removal to obtain a second silver nitrate solution; circulates the second silver nitrate solution between a buffer tank and a high-speed tubular centrifugal device for a third impurity removal to obtain a semi-finished silver nitrate solution; finally, pure nitric acid is used to adjust the pH value of the semi-finished silver nitrate solution to 1-3, and recrystallizes to obtain high-purity silver nitrate. The production process provided by the present invention utilizes the ion exchange, adsorption and chelation of the resin to remove impurity ions, combines filtration and a high-speed tubular centrifugal device to separate fine solid impurities, achieves efficient and thorough removal of impurity ions, and improves the purity of silver nitrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a production process of high-purity silver nitrate, high-purity silver nitrate and applications thereof. Background Art

[0002] Silver powder is widely used in photovoltaic silver paste because of its good conductivity. Photovoltaic silver paste consists of three parts: conductive phase, adhesive phase and organic carrier, among which the conductive phase is the functional phase of photovoltaic silver paste, namely silver powder.

[0003] The key technology for preparing fine silver powder is to select the appropriate combination of silver salt, reducing agent and reaction conditions to obtain fine silver powder with moderate particle size, uniformity, easy dispersion and controllable morphology. The most commonly used silver salt is silver nitrate, and its quality directly affects the quality and applicability of silver powder. In particular, the conductive silver paste is printed on the surface of silicon material by screen printing technology, and the silver electrode is formed after sintering. The metal ion impurities, especially Cu, Ni, Fe, Cr, etc., have a fast diffusion rate in the silicon matrix, and are easy to diffuse into the silicon matrix during the heat treatment process, thereby affecting the efficiency of semiconductor devices.

[0004] The core of the current silver nitrate preparation process is the removal of metal ions, which is generally done by increasing the pH value of the solution to hydrolyze metal ions, especially heavy metal ions, and remove them through adsorption by various adsorbents combined with filtration. This removal method has two problems:

[0005] 1. The selectivity for metal ions is poor and cannot meet the requirements for impurity ion content;

[0006] 2. The solid-liquid separation method has defects, and adsorbed metal ions will still enter the purified solution, causing the quality of the silver nitrate product to decline.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] One of the purposes of the present invention is to provide a production process of high-purity silver nitrate, aiming to solve the technical problems that the preparation process in the prior art has poor selectivity for metal ions and the quality of the silver nitrate product is reduced due to solid-liquid separation.

[0009] A second object of the present invention is to provide a high-purity silver nitrate.

[0010] A third object of the present invention is to provide an application of high-purity silver nitrate.

[0011] In order to solve the above technical problems, the present invention particularly adopts the following technical solutions:

[0012] A first aspect of the present invention provides a production process for high-purity silver nitrate, comprising the following steps:

[0013] A. Heat the silver ingot and concentrated nitric acid to obtain a crude silver nitrate solution with a pH ≥ 3;

[0014] B. adding an adsorption-ion exchange bifunctional resin to the crude silver nitrate solution to perform a first impurity removal and filtering to obtain a first silver nitrate solution;

[0015] C. adding a chelating resin to the first silver nitrate solution to perform a second impurity removal to obtain a second silver nitrate solution; circulating the second silver nitrate solution between a buffer tank and a high-speed tubular centrifuge device to perform a third impurity removal to obtain a semi-finished silver nitrate solution;

[0016] D. Use pure nitric acid to adjust the pH of the semi-finished silver nitrate solution to 1-3, and then perform a crystallization process to obtain the high-purity silver nitrate.

[0017] Furthermore, in step C, the chelating resin is a side chain chelating resin, and the addition amount is 0.3%-2% of the mass of the silver ingot.

[0018] Preferably, the functional groups of the side chain chelating resin include at least one of oximes, 8-hydroxyquinolines and pyridines.

[0019] Preferably, the functional groups of the side chain chelating resin are oximes, 8-hydroxyquinolines and pyridines, and the mass ratio of oximes, 8-hydroxyquinolines and pyridines is 1:(1-2):(1-2).

[0020] Furthermore, in step B, the amount of the adsorption-ion exchange dual-functional resin added is 0.3%-2% of the mass of the silver ingot.

[0021] Furthermore, in step A, the mass fraction of the concentrated nitric acid is 65%-68%.

[0022] Preferably, the added amount of the concentrated nitric acid is 99%-117% of the mass of the silver ingot.

[0023] Furthermore, in step B, an adsorption-ion exchange dual-functional resin is added and stirred for 3 h to 8 h to perform the first impurity removal.

[0024] Preferably, the pH of the first impurity removal is 6.5-7.0, and the time is 5h-10h.

[0025] Furthermore, in step C, a chelating resin is added and stirred for 3 h to 8 h, and then settled for 5 h to 10 h for the second impurity removal.

[0026] Furthermore, in step A, the heating temperature is 80°C-90°C.

[0027] Furthermore, in step D, the crystallization process includes evaporation crystallization followed by cooling crystallization.

[0028] Preferably, when the evaporative crystallization is carried out until a crystal film appears, the process is switched to cooling crystallization.

[0029] Preferably, the method further comprises washing and drying after the crystallization process to obtain the high-purity silver nitrate.

[0030] Preferably, the drying temperature is 60°C-100°C.

[0031] The second aspect of the present invention provides high-purity silver nitrate produced by the production process.

[0032] The third aspect of the present invention provides the use of the high-purity silver nitrate in preparing silver powder for solar cells.

[0033] Compared with the prior art, the present invention has at least the following beneficial effects:

[0034] The production process provided by the present invention utilizes the ion exchange, adsorption and chelation of resin to remove impurity ions, combines filtration and high-speed tubular centrifugal equipment to separate fine solid impurities, achieves efficient and thorough removal of impurity ions, and improves the purity of silver nitrate.

[0035] The high-purity silver nitrate provided by the present invention has a Cu content as low as 0.05 ppb, a Ni content as low as 0.07 ppb, a Fe content as low as 0.17 ppb, and a Cr content as low as 0.07 ppb, and the impurity content is much lower than that of silver nitrate prepared by a conventional method, and the purity is higher.

[0036] The application of the high-purity silver nitrate provided by the present invention provides silver nitrate materials with higher purity for solar cell silver powder, promotes the development of solar cells towards high efficiency and long life, and promotes the rapid development of the downstream industrial chain. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 The process flow chart of high-purity silver nitrate production provided in Example 1. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. The components of the embodiments of the present invention described and shown herein can be arranged and designed in various different configurations.

[0040] A first aspect of the present invention provides a production process for high-purity silver nitrate, comprising the following steps:

[0041] A. Heat the silver ingot and concentrated nitric acid to obtain a crude silver nitrate solution with a pH ≥ 3;

[0042] B. adding an adsorption-ion exchange bifunctional resin to the crude silver nitrate solution to perform a first impurity removal and filtering to obtain a first silver nitrate solution;

[0043] C. adding a chelating resin to the first silver nitrate solution to perform a second impurity removal to obtain a second silver nitrate solution; circulating the second silver nitrate solution between a buffer tank and a high-speed tubular centrifuge device to perform a third impurity removal to obtain a semi-finished silver nitrate solution;

[0044] D. Use pure nitric acid to adjust the pH of the semi-finished silver nitrate solution to 1-3, and then perform a crystallization process to obtain the high-purity silver nitrate.

[0045] The production process provided by the present invention utilizes the ion exchange, adsorption and chelation of resin to remove impurity ions, combines filtration and high-speed tubular centrifugal equipment to separate fine solid impurities, achieves efficient and thorough removal of impurity ions, and improves the purity of silver nitrate.

[0046] In the first separation, a filter element or filter membrane made of PP material is used for filtering in step B to remove most of the solid impurities; in the second separation, the second silver nitrate solution is loaded into a storage tank, and the second silver nitrate solution enters a tubular high-speed centrifuge through a pump. The trace solid impurities gradually diffuse and adhere to the inner surface of the centrifuge cylinder under the action of centrifugal force. The second silver nitrate solution flows back into the storage tank through the overflow port of the centrifuge, and circulates repeatedly between the centrifuge and the storage tank until the impurity ions in the central control solution are qualified, the impurities are enriched in the centrifuge, and a pure silver nitrate solution is obtained in the storage tank.

[0047] In some preferred embodiments of the present invention, in step D, the grade of pure nitric acid is high grade.

[0048] Furthermore, in step C, the chelating resin is a side chain chelating resin, and the addition amount is 0.3%-2% of the mass of the silver ingot.

[0049] The chelate resin is used to carry out targeted secondary impurity removal of impurity ions such as Cu, Ni, Fe, Cr, etc. that diffuse rapidly in the silicon base in the first silver nitrate solution. The chelate resin is a resin with a chelate group, and the chelate resin has a special effect on separating heavy metals and precious metals.

[0050] In some embodiments of the present invention, the added amount of the chelating resin is typically but not limited to 0.3%, 0.6%, 1%, 1.4%, 1.8% or 2% of the mass of the silver ingot.

[0051] Preferably, the functional groups of the side chain chelating resin include at least one of oximes (type I), 8-hydroxyquinolines (type II) and pyridines (type III).

[0052] Among the resins with chelating groups, effective functional groups such as oxime chelating resins can form complexes with metal Ni. The introduction of dioxime groups into the resin skeleton can enhance the activity of Ni. 2+ It has special adsorption properties for metals such as Cr; 8-hydroxyquinoline chelating resin: 2+ 、Ni 2+ 、Zn 2+ It has a special selective adsorption effect on precious metals such as Cu 2+ Cr 3+ 、Ni 2+ The above-mentioned mixture of chelating resins with functional groups is used to chelate and adsorb specific metal ions in the first silver nitrate solution under certain pH conditions.

[0053] Preferably, the functional groups of the side chain chelating resin are oximes, 8-hydroxyquinolines and pyridines, and the mass ratio of oximes, 8-hydroxyquinolines and pyridines is 1:(1-2):(1-2).

[0054] In some embodiments of the present invention, the mass ratio of oxime, 8-hydroxyquinoline and pyridine chelating resins is typically but not limited to 1:1:1, 1:1:2, 1:2:1, 1:2:2, 1:1.5:1.5, 1:1:1.5 or 1:1.5:1.

[0055] Furthermore, in step B, the amount of the adsorption-ion exchange dual-functional resin added is 0.3%-2% of the mass of the silver ingot.

[0056] In some embodiments of the present invention, the addition amount of the adsorption-ion exchange dual-function resin is typically but not limited to 0.3%, 0.6%, 1%, 1.4%, 1.8% or 2% of the mass of the silver ingot.

[0057] Ion exchange resin has enough exchange groups, so it has a higher exchange capacity, while adsorption resin has a very high specific surface area and excellent adsorption performance. This type of bifunctional resin introduces certain functional groups into the macroporous adsorption resin, so it has the dual functions of adsorption and ion exchange.

[0058] In one embodiment of the present invention, the preparation method of the adsorption-ion exchange bifunctional resin is to activate the macroporous bifunctional resin and transform it into a hydroxide type to become a macroporous strong alkaline bifunctional resin with anion exchange capacity. Specifically, on the macroporous polystyrene skeleton, Lewis acid such as ZnCl2, AlCl3, SnCl4, etc. is used for chloromethylation with chloromethyl ether, and then reacted with a quantitative trimethylamine to introduce -N + (CH3)3 groups to obtain a macroporous strong alkaline bifunctional resin with anion exchange capacity. The above adsorption-ion exchange bifunctional resin is added to the crude silver nitrate solution, and the counter ion-hydroxyl on the functional group is exchanged with the nitrate in the solution and enters the solution, which increases the pH value of the solution, partially hydrolyzes the metal ions, and the hydrolysis products are trapped in the pores; at the same time, the polar surface in the pores also has a strong adsorption capacity for high-valent metal ions such as Cu, Ni, Fe, and Cr.

[0059] Furthermore, in step A, the mass fraction of the concentrated nitric acid is 65%-68%.

[0060] Preferably, the amount of concentrated nitric acid added is 94%-117% of the mass of the silver ingot, and the amount of concentrated nitric acid added is 1.1 times-1.3 times the theoretical amount of concentrated nitric acid to ensure that the silver is fully reacted and dissolved.

[0061] Furthermore, in step B, an adsorption-ion exchange dual-functional resin is added and stirred for 3 h to 8 h to perform the first impurity removal.

[0062] Preferably, the pH of the first impurity removal is 6.5-7.0, and the time is 5h-10h.

[0063] Furthermore, in step C, a chelating resin is added and stirred for 3 h to 8 h, and then settled for 5 h to 10 h for the second impurity removal.

[0064] Furthermore, in step A, the heating temperature is 80°C-90°C.

[0065] Furthermore, in step D, the crystallization process includes evaporation crystallization followed by cooling crystallization.

[0066] Preferably, when the evaporative crystallization is carried out until a crystal film appears, the process is switched to cooling crystallization.

[0067] Preferably, the method further comprises washing and drying after the crystallization process to obtain the high-purity silver nitrate.

[0068] Preferably, the drying temperature is 60°C-100°C.

[0069] The second aspect of the present invention provides high-purity silver nitrate produced by the production process.

[0070] The high-purity silver nitrate provided by the present invention has a Cu content as low as 0.05 ppb, a Ni content as low as 0.07 ppb, a Fe content as low as 0.17 ppb, and a Cr content as low as 0.07 ppb, and the impurity content is much lower than that of silver nitrate prepared by a conventional method, and the purity is higher.

[0071] The third aspect of the present invention provides the use of the high-purity silver nitrate in preparing silver powder for solar cells.

[0072] The application of the high-purity silver nitrate provided by the present invention provides silver nitrate materials with higher purity for solar cell silver powder, promotes the development of solar cells towards high efficiency and long life, and promotes the rapid development of the downstream industrial chain.

[0073] In the following, some embodiments of the present invention are described in detail in conjunction with the embodiments. In the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. The raw materials used in the present invention can be obtained by commercial purchase unless otherwise specified.

[0074] The adsorption-ion exchange bifunctional resin used in the following examples and comparative examples is prepared as follows: a macroporous polystyrene skeleton is catalyzed by a Lewis acid such as ZnCl2, AlCl3, SnCl4, etc., and chloromethyl ether is chloromethylated, and then reacted with a quantitative amount of trimethylamine to introduce -N + The (CH3)3 group obtains an adsorption-ion exchange bifunctional resin with anion exchange capacity.

[0075] The oxime chelating resin used in the following examples and comparative examples is TP307; the 8-hydroxyquinoline chelating resin is Chelex 109; and the pyridine chelating resin is D511.

[0076] Example 1

[0077] This embodiment provides a high-purity silver nitrate, and its production process is as follows Figure 1 As shown, the details are as follows:

[0078] (1) Preparation of silver nitrate: 200 kg of silver ingots were washed with dilute nitric acid and added to a reaction kettle, 100 L of pure water and 160 L of 65% concentrated nitric acid were added, and the reaction kettle was heated to 90° C. for reaction. After the reaction was completed, the reaction kettle was heated until the excess nitric acid was completely decomposed to obtain a crude silver nitrate solution with a pH of 3.1;

[0079] (2) Hydrolysis-adsorption removal: Add 1 kg of adsorption-ion exchange bifunctional resin to the crude silver nitrate solution, stir at room temperature for 4 hours, the solution pH value is 6.8, settle for 10 hours, and filter with a 0.2 μm filter element to obtain the first silver nitrate solution;

[0080] (3) Chelation and impurity removal: Add 1 kg of side chain chelating resin to the first silver nitrate solution, wherein the ratio of type I to type II is 1:1. Stir at room temperature for 4 hours and let it settle for 10 hours to obtain a second silver nitrate solution. After removing the resin from the second silver nitrate solution, pump it into a buffer tank and enter a high-speed tubular centrifuge for solid-liquid separation for 50 minutes to obtain a semi-finished silver nitrate solution;

[0081] (4) Evaporation and crystallization: The semi-finished silver nitrate solution is poured into an evaporator, and high-grade pure nitric acid is added to adjust the pH value of the solution to 1. When a crystal film appears on the surface of the solution, the solution is cooled and crystallized. The crystals are centrifuged and washed, and dried at 80°C for 6 hours to obtain high-purity silver nitrate.

[0082] Example 2

[0083] This embodiment provides a high-purity silver nitrate, and its preparation method is as follows:

[0084] (1) Preparation of silver nitrate: 200 kg of silver ingots were washed with dilute nitric acid and then added to a reaction kettle, 100 L of pure water and 150 L of 65% concentrated nitric acid were added, and the reaction kettle was heated and gradually heated to 80° C. for reaction. After the reaction was completed, the reaction kettle was heated until the excess nitric acid was completely decomposed to obtain a crude silver nitrate solution with a pH of 3.2;

[0085] (2) Hydrolysis-adsorption removal: Add 2 kg of adsorption-ion exchange bifunctional resin to the crude silver nitrate solution, stir at room temperature for 4 hours, the solution pH value is 7.0, settle for 10 hours, and filter with a 0.2 μm filter element to obtain the first silver nitrate solution;

[0086] (3) Chelation and impurity removal: Add 1 kg of side chain chelating resin to the first silver nitrate solution, wherein the ratio of type I to type III is 1:2. Stir at room temperature for 4 hours and let it settle for 10 hours to obtain a second silver nitrate solution. After removing the resin from the second silver nitrate solution, pump it into a buffer tank and enter a high-speed tubular centrifuge for solid-liquid separation for 60 minutes to obtain a semi-finished silver nitrate solution;

[0087] (4) Evaporation and crystallization: The semi-finished silver nitrate solution is poured into an evaporator, and high-grade pure nitric acid is added to adjust the pH value of the solution to 1. When a crystal film appears on the surface of the solution, the solution is cooled and crystallized. The crystals are centrifuged and washed, and dried at 80°C for 6 hours to obtain high-purity silver nitrate.

[0088] Example 3

[0089] This embodiment provides a high-purity silver nitrate, and its preparation method is as follows:

[0090] (1) Preparation of silver nitrate: 200 kg of silver ingots were washed with dilute nitric acid and then added to a reaction kettle, 150 L of pure water and 160 L of 65% concentrated nitric acid were added, and the reaction kettle was heated and gradually heated to 90° C. for reaction. After the reaction was completed, the reaction kettle was heated until the excess nitric acid was completely decomposed to obtain a crude silver nitrate solution with a pH of 3.2;

[0091] (2) Hydrolysis-adsorption removal: Add 2 kg of adsorption-ion exchange bifunctional resin to the crude silver nitrate solution, stir at room temperature for 4 hours, the solution pH value is 7.0, settle for 10 hours, and filter with a 0.2 μm filter element to obtain the first silver nitrate solution;

[0092] (3) Chelation and impurity removal: Add 1 kg of side chain chelating resin to the first silver nitrate solution, wherein the mass ratio of type I: type II: type III is 1:1:1. Stir at room temperature for 4 hours and let it settle for 10 hours to obtain a second silver nitrate solution. After removing the resin from the second silver nitrate solution, pump it into a buffer tank and enter a high-speed tubular centrifuge for solid-liquid separation for 60 minutes to obtain a semi-finished silver nitrate solution;

[0093] (4) Evaporation and crystallization: The semi-finished silver nitrate solution is poured into an evaporator, and high-grade pure nitric acid is added to adjust the pH value of the solution to 1. When a crystal film appears on the surface of the solution, the solution is cooled and crystallized. The crystals are centrifuged and washed, and dried at 80°C for 6 hours to obtain high-purity silver nitrate.

[0094] Example 4

[0095] This embodiment provides a high-purity silver nitrate, and its preparation method is as follows:

[0096] (1) Preparation of silver nitrate: same as the step in Example 3;

[0097] (2) Hydrolysis-adsorption impurity removal: add 0.6 kg of adsorption-ion exchange bifunctional resin to the crude silver nitrate solution, stir at room temperature for 4 hours, the solution pH value is 7.0, settle for 10 hours, and filter with a 0.2 μm filter element to obtain the first silver nitrate solution;

[0098] (3) Chelating and removing impurities: the same as the step in Example 3;

[0099] (4) Evaporation and crystallization: Same as the step in Example 3.

[0100] Example 5

[0101] This embodiment provides a high-purity silver nitrate, and its preparation method is as follows:

[0102] (1) Preparation of silver nitrate: same as the step in Example 3;

[0103] (2) Hydrolysis-adsorption removal: Add 4 kg of adsorption-ion exchange bifunctional resin to the crude silver nitrate solution, stir at room temperature for 4 hours, the solution pH value is 7.0, settle for 10 hours, and filter with a 0.2 μm filter element to obtain the first silver nitrate solution;

[0104] (3) Chelating and removing impurities: the same as the step in Example 3;

[0105] (4) Evaporation and crystallization: Same as the step in Example 3.

[0106] Example 6

[0107] This embodiment provides a high-purity silver nitrate, and its preparation method is as follows:

[0108] (1) Preparation of silver nitrate: same as the step in Example 1;

[0109] (2) Hydrolysis-adsorption impurity removal: the same as the step in Example 1;

[0110] (3) Chelation and impurity removal: Add 0.6 kg of side chain chelating resin to the first silver nitrate solution, wherein the ratio of type I to type III is 1:2. Stir at room temperature for 4 hours and let it settle for 10 hours to obtain a second silver nitrate solution. After removing the resin from the second silver nitrate solution, pump it into a buffer tank and enter a high-speed tubular centrifuge for solid-liquid separation for 60 minutes to obtain a semi-finished silver nitrate solution;

[0111] (4) Evaporation and crystallization: Same as the step in Example 1.

[0112] Example 7

[0113] This embodiment provides a high-purity silver nitrate, and its preparation method is as follows:

[0114] (1) Preparation of silver nitrate: same as the step in Example 1;

[0115] (2) Hydrolysis-adsorption impurity removal: the same as the step in Example 1;

[0116] (3) Chelation and impurity removal: Add 4 kg of side chain chelating resin to the first silver nitrate solution, wherein the ratio of type I to type III is 1:2. Stir at room temperature for 4 hours and let it settle for 10 hours to obtain a second silver nitrate solution. After removing the resin from the second silver nitrate solution, pump it into a buffer tank and enter a high-speed tubular centrifuge for solid-liquid separation for 60 minutes to obtain a semi-finished silver nitrate solution;

[0117] (4) Evaporation and crystallization: Same as the step in Example 1.

[0118] Comparative Example 1

[0119] This comparative example provides a silver nitrate, and its preparation method is as follows:

[0120] (1) Preparation of silver nitrate: 200 kg of silver ingots were washed with dilute nitric acid and then added to a reaction kettle, 150 L of pure water and 160 L of 65% concentrated nitric acid were added, and the reaction kettle was heated and gradually heated to 90° C. for reaction. After the reaction was completed, the reaction kettle was heated until the excess nitric acid was completely decomposed to obtain a crude silver nitrate solution with a pH of 3.3;

[0121] (2) Sedimentation and impurity removal: The crude silver nitrate solution was allowed to settle for 4 hours and filtered. The obtained filtrate was heated to 90°C, and 0.5 kg of ferric nitrate as an impurity remover was added under stirring. Then 0.6 kg of silver oxide was added until the pH value of the solution was 6.5. The solution was stirred at this temperature for 1 hour, and filtered after settling for 4 hours.

[0122] (3) Evaporation and crystallization: The filtered silver nitrate solution is poured into an evaporator, and high-grade pure nitric acid is added to adjust the pH value of the solution to 1. The solution is evaporated until a crystal film appears on the surface of the solution, and then cooled and crystallized. The crystals are centrifuged and washed, and dried at 80°C for 6 hours to obtain silver nitrate.

[0123] Comparative Example 2

[0124] This comparative example provides a silver nitrate, and its preparation method is as follows:

[0125] (1) Preparation of silver nitrate: 200 kg of silver ingots were washed with dilute nitric acid and added to a reaction kettle, 100 L of pure water and 160 L of 65% concentrated nitric acid were added, and the reaction kettle was heated to 90° C. for reaction. After the reaction was completed, the reaction kettle was heated until the excess nitric acid was completely decomposed to obtain a crude silver nitrate solution with a pH of 3.1;

[0126] (2) Hydrolysis-adsorption removal: Add 1 kg of adsorption-ion exchange bifunctional resin to the crude silver nitrate solution, stir at room temperature for 4 hours, the solution pH value is 6.8, settle for 10 hours, and filter with a 0.2 μm filter element to obtain the first silver nitrate solution;

[0127] (3) Evaporation and crystallization: The first silver nitrate solution is poured into an evaporating kettle, and high-grade pure nitric acid is added to adjust the pH value of the solution to 1. The solution is evaporated until a crystal film appears on the surface of the solution, and then cooled and crystallized. The crystals are centrifuged and washed, and dried at 80° C. for 6 hours to obtain silver nitrate.

[0128] Comparative Example 3

[0129] This comparative example provides a silver nitrate, and its preparation method is as follows:

[0130] (1) Preparation of silver nitrate: 200 kg of silver ingots were washed with dilute nitric acid and then added to a reaction kettle, 100 L of pure water and 160 L of 65% concentrated nitric acid were added, and the reaction kettle was heated and gradually heated to 90° C. for reaction. After the reaction was completed, the reaction kettle was heated until the excess nitric acid was completely decomposed to obtain a crude silver nitrate solution with a pH of 3.3;

[0131] (2) Chelating and removing impurities: Add 1 kg of side chain chelating resin to the crude silver nitrate solution, wherein the ratio of type I to type II is 1:1. Stir at room temperature for 4 hours and let it settle for 10 hours to obtain a second silver nitrate solution. After removing the resin from the second silver nitrate solution, pump it into a buffer tank and enter a high-speed tubular centrifuge for solid-liquid separation for 60 minutes to obtain a semi-finished silver nitrate solution;

[0132] (3) Evaporation and crystallization: The first silver nitrate solution is poured into an evaporating kettle, and high-grade pure nitric acid is added to adjust the pH value of the solution to 1. The solution is evaporated until a crystal film appears on the surface of the solution, and then cooled and crystallized. The crystals are centrifuged and washed, and dried at 80° C. for 6 hours to obtain silver nitrate.

[0133] Test Example 1

[0134] The silver nitrate obtained in Examples 1-6 and Comparative Examples 1-3 was tested for purity using an inductively coupled plasma mass spectrometer. The data obtained are shown in Table 1.

[0135] Table 1

[0136]

[0137]

[0138] As can be seen from Table 1, by applying the technical method of the present invention, the content of metal impurity ions in the obtained silver nitrate product is significantly reduced. The impurity content of the high-purity silver nitrate prepared by the method of the present invention is much lower than that of the silver nitrate prepared by the conventional method, and it has a particularly good removal effect on the impurity ions such as Cu, Ni, Fe, Cr, etc. that affect the application of solar cell silver powder.

[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A production process for high-purity silver nitrate, characterized in that, The following steps are involved: A. Heat the silver ingot and concentrated nitric acid to obtain a crude silver nitrate solution with a pH ≥ 3; B. adding an adsorption-ion exchange bifunctional resin to the crude silver nitrate solution to perform a first impurity removal and filtering to obtain a first silver nitrate solution; C. adding a chelating resin to the first silver nitrate solution to perform a second impurity removal to obtain a second silver nitrate solution; The second silver nitrate solution is circulated between a buffer tank and a high-speed tubular centrifugal device to perform a third impurity removal to obtain a semi-finished silver nitrate solution; D. Using pure nitric acid to adjust the pH of the semi-finished silver nitrate solution to 1-3, and then performing a crystallization process to obtain the high-purity silver nitrate; In step C, the chelating resin is a side chain chelating resin, and the functional groups of the side chain chelating resin include at least one of oximes, 8-hydroxyquinolines and pyridines.

2. The production process according to claim 1, characterized in that: In step C, the added amount of the chelating resin is 0.3%-2% of the mass of the silver ingot.

3. The production process according to claim 1, characterized in that: The functional groups of the side chain chelating resin are oxime, 8-hydroxyquinoline and pyridine; The mass ratio of oximes, 8-hydroxyquinolines and pyridines is 1:(1-2):(1-2).

4. The production process according to claim 1, characterized in that: The adsorption-ion exchange bifunctional resin is obtained by activating a macroporous bifunctional resin and transforming it into a hydroxide type, thereby becoming a macroporous strongly alkaline bifunctional resin with anion exchange capability.

5. The production process according to claim 1, characterized in that: In step B, the amount of the adsorption-ion exchange dual-functional resin added is 0.3%-2% of the mass of the silver ingot.

6. The production process according to any one of claims 1 to 5, characterized in that: In step A, the mass fraction of concentrated nitric acid is 65%-68%.

7. The production process according to any one of claims 1 to 5, characterized in that: The added amount of the concentrated nitric acid is 99%-117% of the mass of the silver ingot.

8. The production process according to any one of claims 1 to 5, characterized in that: In step B, the first impurity removal is performed by adding an adsorption-ion exchange dual-functional resin and stirring for 3 h to 8 h.

9. The production process according to any one of claims 1 to 5, characterized in that: The pH of the first impurity removal is 6.5-7.0, and the time is 5h-10h.

10. The production process according to any one of claims 1 to 5, characterized in that: In step C, chelating resin is added and stirred for 3h-8h, and then the mixture is allowed to settle for 5h-10h for the second impurity removal.

11. The production process according to any one of claims 1 to 5, characterized in that: In step A, the heating temperature is 80°C-90°C.

12. The production process according to any one of claims 1 to 5, characterized in that: In step D, the crystallization process includes evaporation crystallization followed by cooling crystallization.

13. The production process according to claim 12, characterized in that: When the evaporative crystallization proceeds to the point where a crystal film appears, it is transferred to cooling crystallization.

14. The production process according to any one of claims 1 to 5, characterized in that: The method also includes washing and drying after the crystallization process to obtain the high-purity silver nitrate.

15. The production process according to claim 14, characterized in that: The drying temperature is 60°C-100°C.

16. High-purity silver nitrate produced according to the production process according to any one of claims 1 to 15.

17. Use of the high-purity silver nitrate according to claim 16 in preparing silver powder for solar cells.