Cement slurry system and preparation method suitable for cement plugging in large-slope sections and horizontal sections

By adding spherical water-absorbing gel and fly ash to the cement slurry, the water-cement ratio is adjusted, and combined with water loss reduction agent and retarder, the low viscosity, low volume shrinkage and strong cement plugs in the large slope and horizontal sections are solved. Thixotropic performance issues achieve efficient cement plug sealing effect.

CN116496030BActive Publication Date: 2024-11-08CHINA NAT PETROLEUM CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210054563.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-18
Publication Date
2024-11-08
Estimated Expiration
2042-01-18

AI Technical Summary

Technical Problem

The existing cement slurry system cannot meet the requirements of low viscosity, low volume shrinkage and strong thixotropic performance of cement plugs in large slope and horizontal sections at the same time, resulting in low construction success rate and poor sealing performance.

Method used

Using a cement slurry system containing spherical water-absorbing gel, the water-cement ratio is regulated to above 0.48, combined with fly ash and microsilicon, and water-reducing agent and retarder are used to achieve low viscosity, low volume shrinkage and strong thixotropic properties. .

Benefits of technology

Effectively prevent the chemical shrinkage of cement stone volume, reduce the viscosity of cement slurry, improve the flow, and improve the sealing quality and construction success rate of cement plugs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116496030B_ABST
    Figure CN116496030B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of oilfield chemistry and oil and gas well cementing materials, and specifically relates to a cement slurry system and preparation method suitable for cement plugging in high-inclination sections and horizontal sections, aiming to solve the problem that the existing cement slurry system cannot simultaneously meet the requirements of low viscosity, low volume shrinkage and strong thixotropy. The present invention provides a cement slurry system suitable for cement plugging in high-inclination sections and horizontal sections, including a gelling system, a fluid loss reducer, a retarder, a spherical water-absorbing gel and water; the total amount of slurry mixing water in the cement slurry system and the water contained in the spherical water-absorbing gel makes the water-cement ratio reach above 0.48. The cement slurry system in the present invention has low viscosity, low volume shrinkage and strong thixotropic properties, meeting the requirements of cement plugging in high-inclination sections and horizontal sections.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield chemistry and oil and gas well cementing materials, and particularly relates to a cement slurry system suitable for cement plugging in high-angle sections and horizontal sections and a preparation method thereof. Background Art

[0002] The cement plugging process is a process technology that replaces a certain amount of cement slurry into a certain part of the casing or wellbore to form a new artificial well bottom that meets the engineering needs or to close a certain well section that meets the process requirements. The cement plugging process technology is encountered in drilling, completion construction, downhole operations, and well repair. Cement plugging is a common construction process in downhole operations. With the development of oil fields, especially in the middle and late stages of oil and water well development, the implementation of reservoir transformation, oil production and injection increase measures cannot be separated from cement plugging construction. The main uses of cement plugging in downhole operations are as follows: (1) Seal the new layer on the tested oil layer for oil testing, or seal the non-target layer during stratified operations; (2) Seal the bottom water layer; (3) Find and seal leaks, find and seal channeling, and test the upper casing pressure to isolate and seal a certain layer section; (4) Block abandoned wells and backfill depleted layers; (5) Seal layers for safety purposes (such as sealing high-pressure layers and toxic and harmful fluid layers), etc.

[0003] It is quite difficult to drive a cement plug with high density and small amount of slurry on top of a large amount of liquid with low density in the well. In view of the low success rate of conventional cement plug construction, various research institutions and construction units are constantly developing new process technologies and downhole tools to meet the needs of different site conditions. Among them, the cement slurry system is one of the key factors that determine the quality of cement plugs. Due to the special well types of high-inclination sections and horizontal sections, high performance requirements are placed on the cement slurry used for cement plugs. In order to ensure the effective sealing performance of the cement plug and prevent the occurrence of high-side sealing leakage channels, the cement slurry system is required to have zero water separation, high sedimentation stability, and no shrinkage of the cement stone volume; at the same time, since cement plugs often use fine tubes to inject cement slurry, in order to smoothly implement cement plug construction, the friction resistance during cement injection must be low, so the cement slurry system is required to have low viscosity; but low-viscosity cement slurry will flow along the lower well wall during the waiting process in the high-inclination section and horizontal section, please refer to Figure 2 As shown, it affects the quality of cement plug, so the cement slurry is also required to have strong thixotropic properties.

[0004] Water separation, sedimentation stability, and fluidity are ultimately about controlling the water in cement slurry. If the amount of water added is small, the free water is reduced and the sedimentation stability is improved, but the fluidity of the cement slurry is affected, and a large amount of drag reducer needs to be added; if the amount of water added is large, the fluidity of the cement slurry is improved, but the water absorption and sedimentation stability of the cement slurry are difficult to control. By comparison, it can be found that reducing the amount of water used in cement slurry is beneficial to both water separation and sedimentation stability, and the lost fluidity can be compensated by increasing the amount of drag reducer. However, reducing the amount of water added is likely to cause the volume of cement paste to shrink. Statistics show that when the water-cement ratio is less than 0.4, the volume of cement paste will show obvious self-shrinkage. Taking the 0.44 water-cement ratio commonly used in the cementing industry as an example, when the water loss is 50ml, the remaining water-cement ratio in the cement slurry is only 0.35, and the cement slurry will undergo severe self-shrinkage. Only when the water-cement ratio reaches above 0.48, when the water loss is 50ml, can the remaining water-cement ratio in the cement slurry reach 0.4. However, excessively high water-cement ratio in horizontal wells increases the risk of water separation and sedimentation.

[0005] Low viscosity and thixotropy are a pair of contradictory properties. Usually, the realization of thixotropy requires increasing the viscosity of cement slurry to a certain extent. However, cement plugs are usually constructed with small inner diameter pipes, which require low slurry viscosity to reduce friction. However, low viscosity of cement slurry is easy to mix with drilling fluid underground and flow along the well wall, affecting the sealing performance of cement plugs.

[0006] The cement plugs in highly deviated or horizontal well sections require low viscosity, low volume shrinkage and strong thixotropy in cement slurry performance. The existing cement slurry systems can hardly meet the above requirements. Summary of the invention

[0007] The present invention provides a cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections, so as to effectively solve the problem that the existing cement slurry system cannot simultaneously meet the requirements of low viscosity, low volume shrinkage and strong thixotropy. In order to alleviate the above technical problems, the technical solution provided by the present invention is:

[0008] A cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections comprises a gelling system, a fluid loss reducing agent, a retarder, a spherical water-absorbing gel and water; the total amount of the mixing water in the cement slurry system and the water contained in the spherical water-absorbing gel makes the water-cement ratio reach above 0.48.

[0009] The water-cement ratio of the cement slurry system is above 0.48, which can effectively prevent the chemical shrinkage of the cement stone volume. At the same time, the excess water in the cement slurry is regulated by the spherical water-absorbing gel, and the viscosity of the cement slurry is effectively reduced, the shrinkage of the cement stone is prevented, and the occurrence of unstable slurry results such as water separation and sedimentation is prevented. In addition, due to the "ball effect", the spherical water-absorbing gel can significantly reduce the viscosity of the cement slurry and improve the fluidity of the cement slurry. The spherical water-absorbing gel can also be used as a thixotropic agent, which can enable the cement slurry system to achieve a better thixotropic effect. Therefore, the cement slurry system in the present invention has low viscosity, low volume shrinkage and strong thixotropic properties, which meet the requirements of cement plugging in large-slope sections and horizontal sections.

[0010] Furthermore, the cementitious system is composed of the following components and their weight parts: 100 parts of oil well cement, 25-30 parts of fly ash (sinking beads), and 5-10 parts of microsilica; preferably, the oil well cement is Class D oil well cement.

[0011] Microsilica and fly ash are both extremely fine spherical particles with significant hydration and consume a large amount of water. When left static or under low shear, the cement slurry will show a macroscopic viscosity increase phenomenon due to the absorption of a large amount of water. Under high-speed shear, it can also show a ball effect and reduce viscosity. Therefore, the combination of fly ash (sinking beads) and microsilica gives the cement slurry certain thixotropic properties, thereby preventing the cement slurry from scattering and flowing along the lower well wall during the setting process, which is of great significance to improving the sealing quality of cement plugs in highly inclined and horizontal well sections.

[0012] Furthermore, the spherical hydrogel has a water content of 22±5 g / g. The hydrogel sphere diameter is 50 to 250 μm. The spherical hydrogel is prepared by an inverse suspension polymerization method, specifically according to the preparation method in Chinese patent CN111807747A, and is specifically a spherical hydrogel copolymerized with acrylamide and 2-acrylamido-2-methylpropanesulfonic acid (mass ratio 7:3).

[0013] Furthermore, the amount of the spherical water-absorbing gel is 10%-25% of the mass of the cement.

[0014] The spherical water-absorbing gel prevents the shrinkage of the cement stone itself by physically controlling water. No chemical reaction occurs in the process. Although the water in the cement slurry is physically released, the effect on the performance of the cement slurry is small because of the low amount added and the reasonable design of the water control amount.

[0015] Furthermore, the fluid loss reducer is a copolymerized fluid loss reducer containing 1.5 to 5.0 parts of sulfonic acid groups and carboxylic acid groups.

[0016] Furthermore, the retarder is 0.5 to 5.0 parts of a modified starch type or a copolymerized type retarder of sulfonic acid groups and carboxylic acid groups.

[0017] Furthermore, at 90-120°C, a modified starch type retarder is used; at 120-150°C, a sulfonic acid group and carboxylic acid group copolymer type retarder is used.

[0018] Furthermore, it also includes a sulfonated aldehyde ketone type dispersant, and the amount of the dispersant is 0.25%-2.0% of the mass of the cement.

[0019] A method for preparing the above-mentioned cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections comprises the following steps:

[0020] dry-mixing the fluid loss additive with the gelling system to obtain a solid mixture;

[0021] Adding the spherical water-absorbing gel and the retarder into water and mixing them to obtain a liquid mixture;

[0022] The solid mixture and the liquid mixture are stirred and mixed to obtain a cement slurry system.

[0023] Furthermore, a dispersant is added when preparing the solid mixture.

[0024] In summary, the cement slurry system and preparation method provided in the present invention for cement plugging in steeply inclined sections and horizontal sections have the following beneficial effects:

[0025] 1. The spherical water-absorbing gel plays a role in controlling water and preventing shrinkage in cement slurry. The total amount of water in the cement slurry and the water contained in the spherical water-absorbing gel can make the water-cement ratio reach above 0.48, which can effectively prevent the chemical shrinkage of cement stone volume;

[0026] 2. The water content is controlled by the water-absorbing gel to prevent the occurrence of unstable slurry results such as water separation and sedimentation. In addition, due to the "ball effect", the spherical water-absorbing gel can significantly reduce the viscosity of the cement slurry and improve the fluidity of the cement slurry;

[0027] 3. The spherical water-absorbing gel can also act as a thixotropic agent. At the same time, the combination of fly ash (sinking beads) and micro-silicon makes the cement slurry have better thixotropic properties, preventing the cement slurry from scattering and flowing along the lower well wall during the setting process;

[0028] 4. The density of the cement slurry system ranges from 1.70-1.90g / cm 3 Adjustable. By adjusting the admixtures (fluid loss reducer and retarder), it can meet the requirements of plugging construction under the condition of less than 150℃.

[0029] 5. The preparation method has simple steps and is easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the related technologies, the drawings required for use in the specific embodiments or the related technical descriptions will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 A graph showing the volume change of cement stone when different amounts of spherical water-absorbing gels are added according to an embodiment of the present invention;

[0032] Figure 2 It is the cement slurry casting scattering diagram mentioned in the background technology;

[0033] Figure 3 A cement slurry thickening curve at 100°C provided in an embodiment of the present invention;

[0034] Figure 4 A cement slurry thickening curve at 110°C provided in an embodiment of the present invention;

[0035] Figure 5 A cement slurry thickening curve at 120°C provided in an embodiment of the present invention;

[0036] Figure 6 This is a cement slurry thickening curve at 150°C provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.

[0038] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0039] Example 1 A cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections

[0040] A gelling system consisting of 100 parts of Class D oil well cement, 25 parts of fly ash (sinking beads) and 5 parts of microsilica is dry-mixed with 2.5 parts of sulfonic acid group and carboxylic acid group copolymer type fluid loss reducer to obtain a solid mixture; 10 parts of spherical water-absorbing gel and 1.5 parts of sulfonic acid group and carboxylic acid group copolymer type retarder are added to 40 parts of water and mixed to obtain a liquid mixture; the above solid mixture and liquid mixture are stirred and mixed to obtain a cement slurry system, which is marked as C1.

[0041] Example 2 A cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections

[0042] A gelling system consisting of 100 parts of Class D oil well cement, 30 parts of fly ash (sinking beads) and 8 parts of microsilica is dry-mixed with 2 parts of sulfonic acid group and carboxylic acid group copolymer type fluid loss reducer to obtain a solid mixture; 15 parts of spherical water-absorbing gel and 1.5 parts of modified starch type retarder are added to 41 parts of water and mixed to obtain a liquid mixture; the above solid mixture and liquid mixture are stirred and mixed to obtain a cement slurry system, which is marked as C2.

[0043] Example 3 A cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections

[0044] A gelling system consisting of 100 parts of Class D oil well cement, 30 parts of fly ash (sinking beads) and 8 parts of microsilica is dry-mixed with 2 parts of sulfonic acid group and carboxylic acid group copolymer type fluid loss reducer to obtain a solid mixture; 20 parts of spherical water-absorbing gel and 2 parts of sulfonic acid group and carboxylic acid group copolymer type retarder are added to 42.4 parts of water and mixed to obtain a liquid mixture; the above solid mixture and liquid mixture are stirred and mixed to obtain a cement slurry system, which is marked as C3.

[0045] Example 4 A cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections

[0046] A gelling system consisting of 100 parts of Class D oil well cement, 30 parts of fly ash (sinking beads) and 8 parts of microsilica is dry-mixed with 2.5 parts of sulfonic acid group and carboxylic acid group copolymer type fluid loss reducer to obtain a solid mixture; 25 parts of spherical water-absorbing gel and 2 parts of sulfonic acid group and carboxylic acid group copolymer type retarder are added to 46.5 parts of water and mixed to obtain a liquid mixture; the above solid mixture and liquid mixture are stirred and mixed to obtain a cement slurry system, which is marked as C4.

[0047] Example 5 Comparative sample (without adding spherical water-absorbing gel)

[0048] A cementitious system consisting of 100 parts of Class D oil well cement, 30 parts of fly ash (sinking beads) and 8 parts of microsilica is dry-mixed with 2.5 parts of sulfonic acid group and carboxylic acid group copolymer type fluid loss reducer to obtain a solid mixture; 1.5 parts of sulfonic acid group and carboxylic acid group copolymer type retarder is added to 50 parts of water and mixed to obtain a liquid mixture; the above solid mixture and liquid mixture are stirred and mixed to obtain a cement slurry system, which is marked as C5.

[0049] Example 6 Comparative sample (without adding spherical water-absorbing gel, adding dispersant)

[0050] A gelling system consisting of 100 parts of Class D oil well cement, 30 parts of fly ash (sinking beads) and 8 parts of microsilica is dry-mixed with 2.5 parts of sulfonic acid group and carboxylic acid group copolymer type fluid loss reducer and 0.5 part of sulfonated aldehyde ketone type dispersant to obtain a solid mixture; 1.5 parts of sulfonic acid group and carboxylic acid group copolymer type retarder is added to 50 parts of water and mixed to obtain a liquid mixture; the above solid mixture and liquid mixture are stirred and mixed to obtain a cement slurry system, which is marked as C6.

[0051] Example 7 Comparative sample (without addition of spherical water-absorbing gel, fly ash (sinking beads) and micro-silicon)

[0052] 138 parts of Class D oil well cement, 2.5 parts of sulfonic acid group and carboxylic acid group copolymer type fluid loss reducer, and 0.5 parts of sulfonated aldehyde ketone type dispersant are dry-mixed to obtain a solid mixture; 1.5 parts of sulfonic acid group and carboxylic acid group copolymer type retarder are added to 50 parts of water and mixed to obtain a liquid mixture; the above solid mixture and liquid mixture are stirred and mixed to obtain a cement slurry system, which is marked as C7.

[0053] Performance Test:

[0054] 1. Test the volume change of cement stone

[0055] The cement paste system in Examples 1 to 7 was measured according to ANSI / API Recommended Practice 10B-5. Figure 1 The specific results are as follows:

[0056] After adding spherical water-absorbing gel at a ratio of 10%, 15%, 20% and 25% of the cement mass, the volume of the cement paste did not shrink.

[0057] 2. Cement slurry density, water separation, sedimentation stability, thixotropy and fluidity tests

[0058] The fluidity of cement slurry was measured according to ANSI / API Recommended Practice 10B-5. The sedimentation stability was characterized by the difference between the upper and lower densities of the cement slurry system. The thixotropic performance was characterized by the difference between the final cut and the initial cut.

[0059] Table 1: Test results of cement slurry density, water separation, sedimentation stability, thixotropy and fluidity

[0060] Cement slurry samples <![CDATA[Density g / cm 3 > Water analysis ml <![CDATA[Settlement stability g / cm 3 > Thixotropic properties Fluidity cm C1 1.90 0 0.03 25 24 C2 1.85 0 0.01 26 24 C3 1.80 0 0.006 23 23 C4 1.75 0 0.005 24 23 C5 1.90 1 0.07 25 18 C6 1.90 2 0.1 20 22 C7 1.90 0.5 0.05 2 20

[0061] From the test results in Table 1, it can be seen that after the spherical water-absorbing gel is added to the cement slurry system C1-C4, the cement slurry has excellent water absorption performance and sedimentation stability; the cement slurry system C5 does not add the spherical water-absorbing gel. Compared with the cement slurry systems C1-C4 with the spherical water-absorbing gel, the spherical water-absorbing gel significantly improves the fluidity of the cement slurry, and the fluidity of the cement slurry system C6 with the dispersant is also improved; after adding the dispersant, the fluidity of the cement slurry can meet the requirements, but the sedimentation stability and water separation performance of the cement slurry are destroyed. Compared with the cement slurry system C5 without the spherical water-absorbing gel, the cement slurry system C7 without the combination of fly ash (sinking beads) and microsilicon has a significant decrease in thixotropic performance. It can be seen that the combination of fly ash (sinking beads) and microsilicon can significantly improve the thixotropic performance of the cement slurry.

[0062] 3. Test cement slurry viscosity

[0063] Table 2: Cement slurry six-speed viscometer test results

[0064]

[0065] From the test results in Table 2, it can be seen that the reading at 600 rpm is low, indicating that the viscosity of the cement slurry is low.

[0066] 4. Cement slurry thickening time test

[0067] The thickening time of the cement slurry systems in Examples 1 to 7 was measured at 100°C (Example 2), 110°C (Example 2), 120°C (Example 1) and 150°C (Example 4). Please refer to Figures 3 to 6 , the specific results are as follows:

[0068] The cement slurry system meets the injection plug construction time requirements under conditions within 150°C.

[0069] 5. Cement stone compressive strength test

[0070] Table 3: Cement paste compressive strength test results

[0071]

[0072] From the test results in Table 3, it can be seen that the cement slurry system suitable for cement plugging in steep slope sections and horizontal sections has a compressive strength of cement paste greater than 14 MPa after curing for 24 hours under different conditions.

[0073] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.

Claims

1. A cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections, characterized in that: It includes a gelling system, a fluid loss reducing agent, a retarder, a spherical water-absorbing gel and water; The total amount of the slurry preparation water in the cement slurry system and the water contained in the spherical water-absorbing gel is such that the water-cement ratio reaches 0.48 or more; The gelling system is composed of the following components and their weight parts: 100 parts of oil well cement, 25-30 parts of fly ash beads, and 5-10 parts of microsilica; The fluid loss reducer is a copolymerized fluid loss reducer of 1.5 to 5.0 parts of sulfonic acid groups and carboxylic acid groups; The retarder is 0.5 to 5.0 parts of a modified starch type or a copolymerized type of a sulfonic acid group and a carboxylic acid group.

2. The cement slurry system suitable for cement plugging in high-slope sections and horizontal sections according to claim 1 is characterized in that: The oil well cement is Class D oil well cement.

3. The cement slurry system suitable for cement plugging in high-slope sections and horizontal sections according to claim 1 is characterized in that: The water content of the spherical water-absorbing gel is 22±5 g / g, and the diameter of the hydrogel sphere is 50-250 μm.

4. The cement slurry system suitable for cement plugging in high-slope sections and horizontal sections according to claim 2 is characterized in that: The amount of the spherical water-absorbing gel is 10%-25% of the mass of the cement.

5. The cement slurry system suitable for cement plugging in high-slope sections and horizontal sections according to claim 1 is characterized in that: At 90-120℃, use modified starch type retarder; At 120-150℃, a copolymerized retarder of sulfonic acid group and carboxylic acid group is used.

6. The cement slurry system suitable for cement plugging in high-slope sections and horizontal sections according to claim 2 is characterized in that: The invention also comprises a sulfonated aldehyde-ketone type dispersant, and the dosage of the dispersant is 0.25%-2.0% of the mass of the cement.

7. A method for preparing a cement slurry system suitable for cement plugging in steeply inclined sections and horizontal sections as claimed in claim 6, characterized in that: The steps include: dry-mixing the fluid loss additive with the gelling system to obtain a solid mixture; Adding the spherical water-absorbing gel and the retarder into water and mixing them to obtain a liquid mixture; The solid mixture and the liquid mixture are stirred and mixed to obtain a cement slurry system.

8. The method for preparing a cement slurry system suitable for cement plugging in high-slope sections and horizontal sections according to claim 7, characterized in that: When preparing the solid mixture, the dispersant is also added.