A preparation process of environmentally friendly sewer brick combined with modified phosphate

By combining modified aluminum dihydrogen phosphate with other materials, environmentally friendly sliding spout tiles are prepared, which solves the problems of easy removal of antioxidant materials, heavy equipment cleaning and insufficient environmental protection requirements in traditional production, achieving low cost, high strength and environmental protection. production effect.

CN116535197BActive Publication Date: 2024-10-15HENAN PROVINCE XINTUO REFRACTORY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310404817.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-15
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

The production of traditional sliding nozzle bricks has problems such as easy decarburization and oxidation of antioxidant materials, heavy equipment cleaning, large impact of ambient temperature and humidity, limited shelf life, insufficient environmental protection requirements, harmful volatile pollution and high costs.

Method used

Modified aluminum dihydrogen phosphate is used as an inorganic binder, mixed with high-alumina bauxite, graphite powder and other materials, and a wet mill and press are used to prepare environmentally friendly drain bricks to form a stable mullite phase, improve the strength of the product and Reduce costs.

Benefits of technology

It achieves environmentally friendly, low-cost production, reduces worker labor intensity, reduces equipment cleaning requirements, avoids volatile pollution, improves the strength and qualification rate of products, and meets low-carbon requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004696491530000011
    Figure GDA0004696491530000011
  • Figure GDA0004696491530000021
    Figure GDA0004696491530000021
  • Figure GDA0004696491530000031
    Figure GDA0004696491530000031
Patent Text Reader

Abstract

The invention discloses a preparation process of a modified phosphate-bonded environmentally friendly downspout brick, wherein the main raw materials are: 60-65 parts of aggregate 88-grade high-alumina bauxite particles or corundum particles, 23-28 parts of 88-grade high-alumina bauxite powder or corundum powder, 2-5 parts of 97-grade graphite powder, 1-5 parts of 95-grade metal silicon powder, 2-6 parts of white mud, 2-4 parts of 95-grade silicon carbide powder, 2-5 parts of high-temperature asphalt powder and 3-7 parts of modified dihydrogen aluminum phosphate. The modified dihydrogen aluminum phosphate of the invention can replace the organic binder resin to play a temporary bonding role, and can meet the semi-finished product forming strength requirements of the sliding downspout brick through the chemical bonding mechanism.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sliding nozzle bricks for steelmaking, and in particular relates to a preparation process of environmentally friendly downspout bricks combined with modified phosphates. Background Art

[0002] In order to meet national environmental protection requirements, reducing production costs while ensuring product quality has become the main task of sliding nozzle brick manufacturers.

[0003] Traditional organic binder resin combined drain has the following disadvantages:

[0004] 1. It is necessary to add a variety of antioxidant materials, which are easy to decarbonize and oxidize;

[0005] 2. The cleaning of mixing production equipment is more frequent and the workload is heavy, which increases the labor intensity of workers;

[0006] 3. It is greatly affected by ambient temperature and humidity, and has great limitations when used in different seasons;

[0007] 4. Due to the addition of metal additives, the shelf life is limited and the product is prone to hydration;

[0008] 5. The development trend of environmental protection requirements is carbon-free, and resin is an organic binder;

[0009] 6. The resin contains free phenol and formaldehyde, which are easy to volatilize during mixing, polluting the environment and harmful to the health of employees. It also contains free water and easily forms bound water during use, which affects the performance of the clay and causes the product to crack after drying. 7. The amount added is greatly affected by the season, temperature, and humidity. The larger the amount added, the higher the cost. Summary of the invention

[0010] The technical problem solved by the invention is to provide a preparation process of environmentally friendly drain bricks combined with modified phosphate.

[0011] The present invention adopts the following technical solutions to solve the above technical problems:

[0012] A preparation process of a modified phosphate-bonded environmentally friendly drain brick, characterized by the following specific steps:

[0013] Step S1, weigh the raw materials according to the following weight ratio:

[0014]

[0015] The weighed 88-grade high-alumina bauxite powder or corundum powder, graphite powder, metallic silicon powder, white mud, silicon carbide powder and high-temperature asphalt powder are uniformly mixed to prepare a mixed powder, wherein the modified aluminum dihydrogen phosphate is composed of aluminum dihydrogen phosphate with a specific gravity of ≥1.5, dextrin and oxalic acid;

[0016] Step S2, using an open wet mill or a closed wet mill or a high-speed closed wet mill to first mix the weighed aggregate 88-grade high-alumina bauxite particles or corundum particles for 1-2 minutes, then add 2-5 parts of modified aluminum dihydrogen phosphate and mix for 3-5 minutes, then add the mixed powder and mix for 10-15 minutes, and finally the mixed mud needs to be trapped for 8-24 hours;

[0017] Step S3, the trapped mud is returned to the mill for secondary mixing, and the remaining modified aluminum dihydrogen phosphate is added at the same time, and mixed for 10-15 minutes, and then pressed by a press to form a brick blank, and then shelled after drying and testing, and then dried and baked.

[0018] Further defined, step S1 weighs the raw materials according to the following weight ratio:

[0019]

[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0021] 1. The modified aluminum dihydrogen phosphate used is an inorganic binder, which is easy to produce. It plays a temporary bonding role during molding, and the strength increases at around 200°C. After that, as the use temperature increases during use, the bonding strength shows an increasing trend, and can reach a peak at 1250°C.

[0022] 2. It can replace organic binder resin to play a temporary bonding role. Through the chemical bonding mechanism, it can meet the molding strength requirements of the semi-finished sliding nozzle bricks.

[0023] 3. During the heating process of the products bonded with the modified binder aluminum dihydrogen phosphate, the strength gradually and evenly increases from low temperature to medium and high temperature, reaching a peak at 1250 degrees. Before reaching the peak, the substances in the mud have formed a crystalline phase such as mullite phase through in-situ sintering reaction, and the strength of the product itself is improved, so that the strength of the product and the strength of the binder can be transferred like a baton, ensuring the strength of the product.

[0024] 4. The binder itself will not cause oxidation, which will cause the product structure to collapse and be damaged during use; antioxidant substances can be reduced, removed or replaced as needed, which can effectively reduce the cost of raw materials and meet environmental protection and low-carbon requirements.

[0025] 5. The requirements for mixing equipment are low and easy to clean. The mixed clay is more operable than the resin-bonded clay; the influence of environmental factors (temperature, humidity) is basically zero; the binder itself has no volatile matter and will not cause environmental problems. The amount added is less than that of resin and it is stable. Price advantage: aluminum dihydrogen phosphate (4000-4500 yuan / t), thermosetting phenolic resin (12000-13500 yuan / t). DETAILED DESCRIPTION

[0026] The specific technical solutions of the present invention are described in detail in conjunction with specific embodiments.

[0027] Example 1

[0028] Step S1, weigh the raw materials according to the following weight ratio:

[0029]

[0030] The weighed 88-grade high-alumina bauxite powder or corundum powder, graphite powder, metallic silicon powder, white mud, silicon carbide powder and high-temperature asphalt powder are uniformly mixed to prepare a mixed powder, wherein the modified aluminum dihydrogen phosphate is composed of 3 parts of aluminum dihydrogen phosphate with a specific gravity ≥1.5, 0.5 parts of yellow dextrin and 0.5 parts of oxalic acid;

[0031] Step S2, using an open wet mill or a closed wet mill or a high-speed closed wet mill to first mix the weighed aggregate 88-grade high-alumina bauxite particles or corundum particles for 1-2 minutes, then add 4 parts of modified aluminum dihydrogen phosphate and mix for 3-5 minutes, then add the mixed powder and mix for 10-15 minutes, and finally the mixed mud needs to be trapped for 8-24 hours;

[0032] Step S3, the trapped mud is returned to the mill for secondary mixing, and the remaining modified aluminum dihydrogen phosphate is added at the same time, and mixed for 10-15 minutes, and then pressed by a press to form a brick blank, and then shelled after drying and testing, and then dried and baked.

[0033] Example 2

[0034] Step S1, weigh the raw materials according to the following weight ratio:

[0035]

[0036]

[0037] The weighed 88-grade high-alumina bauxite powder or corundum powder, graphite powder, metallic silicon powder, white mud, silicon carbide powder and high-temperature asphalt powder are uniformly mixed to prepare a mixed powder, wherein the modified aluminum dihydrogen phosphate is composed of 2.5 parts of aluminum dihydrogen phosphate with a specific gravity ≥1.5, 0.3 parts of dextrin and 0.2 parts of oxalic acid;

[0038] Step S2, using an open wet mill or a closed wet mill or a high-speed closed wet mill to first mix the weighed aggregate 88-grade high-alumina bauxite particles or corundum particles for 1-2 minutes, then add 2 parts of modified aluminum dihydrogen phosphate and mix for 3-5 minutes, then add the mixed powder and mix for 10-15 minutes, and finally the mixed mud needs to be trapped for 8-24 hours;

[0039] Step S3, the trapped mud is returned to the mill for secondary mixing, and the remaining modified aluminum dihydrogen phosphate is added at the same time, and mixed for 10-15 minutes, and then pressed by a press to form a brick blank, and then shelled after drying and testing, and then dried and baked.

[0040] Example 3

[0041] Step S1, weigh the raw materials according to the following weight ratio:

[0042]

[0043] The weighed 88-grade high-alumina bauxite powder or corundum powder, graphite powder, metallic silicon powder, white mud, silicon carbide powder and high-temperature asphalt powder are uniformly mixed to prepare a mixed powder, wherein the modified aluminum dihydrogen phosphate is composed of 5 parts of aluminum dihydrogen phosphate with a specific gravity ≥1.5, 1 part of dextrin and 1 part of oxalic acid;

[0044] Step S2, using an open wet mill or a closed wet mill or a high-speed closed wet mill to first mix the weighed aggregate 88-grade high-alumina bauxite particles or corundum particles for 1-2 minutes, then add 5 parts of modified aluminum dihydrogen phosphate and mix for 3-5 minutes, then add the mixed powder and mix for 10-15 minutes, and finally the mixed mud needs to be trapped for 8-24 hours;

[0045] Step S3, the trapped mud is returned to the mill for secondary mixing, and the remaining modified aluminum dihydrogen phosphate is added at the same time, and mixed for 10-15 minutes, and then pressed by a press to form a brick blank, and then shelled after drying and testing, and then dried and baked.

[0046] The inspection indicators of the drain bricks prepared in Example 1 are shown in Table 1.

[0047] Table 1

[0048]

[0049] (1) After replacing the resin binder, it meets environmental protection requirements and takes a big step towards low-carbon and carbon-free production;

[0050] (2) Reduce the labor intensity of workers; the equipment runs more smoothly, reducing the number of times and time spent on cleaning and forging the mill;

[0051] (3) The frequency of process product failures is significantly reduced, and the pass rate is significantly improved;

[0052] (4) The binder alone directly reduced the company's production costs by RMB 1.4242 million, as shown in Table 2.

[0053] Table 2

[0054]

[0055] The basic principles, main features and advantages of the present invention are shown and described above. Without departing from the spirit and scope of the present invention, the present invention may also be subject to various changes and improvements, which all fall within the scope of the present invention to be protected.

Claims

1. A process for preparing a modified phosphate-bonded environmentally friendly drain brick, characterized in that The specific steps are: Step S1, weigh the raw materials according to the following weight ratio: 88 grade high alumina particles or corundum particles 5mm 60-65 parts 88 grade high alumina powder or corundum powder 180 mesh 23-28 parts 97 graphite powder 100 mesh 2-5 parts 95 Metal Silicon Powder 325 Mesh 1-5 parts 2-6 portions of white mud 180 mesh 95 Silicon carbide powder 180 mesh 2-4 parts High temperature asphalt powder 100 mesh 2-5 parts 3-7 parts of modified aluminum dihydrogen phosphate The weighed 88-grade high-alumina bauxite powder or corundum powder, graphite powder, metallic silicon powder, white mud, silicon carbide powder and high-temperature asphalt powder are uniformly mixed to form a mixed powder, wherein the modified aluminum dihydrogen phosphate is composed of 4-6 parts by weight of aluminum dihydrogen phosphate with a specific gravity ≥1.5, 0.5-1.5 parts by weight of dextrin and 0.5-1.5 parts by weight of oxalic acid; Step S2, using an open wet mill, a closed wet mill or a high-speed closed wet mill, firstly mix the weighed 88-grade high-alumina bauxite particles or corundum particles for 1-2 minutes, then add 2-5 parts of modified aluminum dihydrogen phosphate and mix for 3-5 minutes, then add the mixed powder and mix for 10-15 minutes, and finally the mixed mud needs to be trapped for 8-24 hours; Step S3, the trapped mud is returned to the mill for secondary mixing, and the remaining modified aluminum dihydrogen phosphate is added at the same time, and mixed for 10-15 minutes, and then pressed into a brick blank using a press of ≥630t, and then shelled after being dried and tested for compliance, and then dried and baked.

2. The process for preparing a modified phosphate-bonded environmentally friendly drain brick according to claim 1, characterized in that Step S1: weigh the raw materials according to the following weight ratio: 88 grade high alumina particles or corundum particles 5mm 62 parts 88 grade high alumina powder or corundum powder 180 mesh 25 parts 97 graphite powder 100 mesh 4 parts 95 Metal Silicon Powder 325 Mesh 3 Pieces 4 parts of white mud 180 mesh 95 Silicon carbide powder 180 mesh 3 parts High temperature asphalt powder 100 mesh 3 parts 4 parts of modified aluminum dihydrogen phosphate.