Organic-inorganic hybrid salt-resistant superabsorbent resin and its preparation

By modifying coal mine waste into an organic-inorganic hybrid superabsorbent resin, the problems of insufficient water release capacity and poor salt tolerance of existing resins in extreme environments have been solved, achieving efficient soil improvement and cost reduction.

CN116554387BActive Publication Date: 2024-11-26NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310617525.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-26
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

Existing superabsorbent resins have limited water release capacity in extremely dry environments and poor salt resistance, which affects their application in the improvement of desert and saline-alkali soils, and their production costs are high.

Method used

An organic-inorganic hybrid superabsorbent resin modified with coal mine waste residue was developed. By introducing coal mine waste residue and organic components into the polymerization stage to crosslink, a uniform gel product was formed, which optimized the network structure of the resin and improved its salt resistance and water absorption.

Benefits of technology

It significantly improves the water retention stability and water absorption effect of the resin, reduces production costs, and enhances its application effect in saline-alkali land and saline soil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116554387B_ABST
    Figure CN116554387B_ABST
Patent Text Reader

Abstract

An organic-inorganic hybrid salt-resistant super absorbent resin is characterized in that it includes the following components in parts by weight: 1-10 parts of linear monomers, 1-5 parts of salt-resistant functional monomers, 0.02-0.20 parts of cross-linking monomers, 0.05-0.15 parts of initiators, and 0.3-1.0 parts of coal mine waste slag; the linear monomers are two or three of methacrylic acid, acrylic acid, and acrylamide; the salt-resistant functional monomers are 2-acrylamide-2-methylpropanesulfonic acid and / or N-vinyl pyrrolidone; the cross-linking monomers use one or more of N,N-methylenebisacrylamide, pentaerythritol triacrylate, and pentaerythritol tetraacrylate; the initiator is ammonium persulfate. Coal mine waste slag is added to the polymer network of the resin as a cross-linking component, so that the super absorbent resin significantly optimizes the surface structure, generates a large number of pore structures, and thus greatly improves its water absorption rate. At the same time, the waste slag, as an inorganic mineral, improves the overall salt resistance of the resin, optimizes its effect of releasing absorbed water, and reduces the cost of producing super absorbent resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of super absorbent resins, and specifically relates to an organic-inorganic hybrid salt-resistant super absorbent resin cross-linked and modified by coal mine waste slag. Background Art

[0002] Superabsorbent resin (SAR), a polymer material that can absorb hundreds or even thousands of times its own weight of water, has a fast water absorption rate and good water retention performance. It has been widely used in agriculture, health, construction and many other fields. In particular, the existing water-absorbing resins used in agriculture still have many defects, such as high production cost of water-absorbing resins, poor salt tolerance, poor water release performance and poor plant compatibility, which seriously affect the application of water-absorbing resins. In soil remediation and soil improvement, although water-absorbing resins with strong water absorption performance can absorb a large amount of water, in some extremely dry environments, such as desert environments, due to the limited water release capacity of water-absorbing resins, they cannot release water well to supply surrounding plants, and their application is limited. The use of sodium-alkali neutralized water-absorbing resins also has an adverse effect on plant growth. Moreover, due to the salt water resistance of water-absorbing resins, the application effect in similar saline-alkali land or saline soil drops sharply, and their water retention performance cannot be fully utilized. Therefore, the development of water-absorbing resins with low cost, potassium-alkali neutralization, good salt tolerance and good water release performance is crucial for soil improvement, especially for desert soil and saline-alkali land soil improvement.

[0003] Organic-inorganic hybrid modified water-absorbing resin is a major development direction of water-absorbing resin. However, usually inorganic components such as zeolite, bentonite, diatomaceous earth, sepiolite and other components are used for hybrid modification, often in the form of mixed fillers with water-absorbing resin, which results in no effective combination of organic and inorganic components, and the water absorption and water retention effects are relatively poor.

[0004] One of the main ways to deal with the large amount of coal mine waste in my country is to make full use of the waste as an additive component of high-value products. Using coal mine waste as an efficient water storage material has achieved its high-value utilization, and the high specific surface area of ​​the waste has a good adsorption effect on ionic brine.

[0005] There is a lack of research on organic-inorganic hybrid water-absorbing resins modified by coal mine waste residue in China. With the excellent adsorption effect of waste residue on ionic media and the good water absorption and salt resistance of organic water-absorbing resins, water-absorbing and water-retaining materials with good improvement effects on saline-alkali land and saline soil can be prepared. Due to the use of cheap waste residue materials, the cost of the modified water-absorbing resin is relatively low. And due to the implementation of organic-inorganic hybrid methods, the cross-linking structure of the water-absorbing resin can be fully optimized, and the salt resistance, water absorption efficiency, and water release effect can be improved. Summary of the invention

[0006] In order to optimize and solve the above problems, the present invention provides an organic-inorganic hybrid salt-resistant super absorbent resin prepared and modified by coal mine waste slag, and a specific preparation method thereof.

[0007] The invention provides an organic-inorganic hybrid salt-resistant super absorbent resin, comprising the following components in parts by weight: 1-10 parts of a linear monomer, 1-5 parts of a salt-resistant functional monomer, 0.02-0.20 parts of a cross-linking monomer, 0.05-0.15 parts of an initiator, and 0.3-1.0 parts of coal mine waste slag, wherein the metal content of the coal mine waste slag is 0.003 µg / g of mercury, 30.8 µg / g of lead, 3.30 µg / g of cadmium, 887 µg / g of barium, and 390 µg / g of Sr. The linear monomer is two or three of methacrylic acid, acrylic acid, and acrylamide. The salt-resistant functional monomer is 2-acrylamide-2-methylpropanesulfonic acid and / or N-vinyl pyrrolidone. The cross-linking monomer uses one or more of N,N-methylenebisacrylamide, pentaerythritol triacrylate, and pentaerythritol tetraacrylate. The initiator is ammonium persulfate.

[0008] The preparation of organic-inorganic hybrid salt-resistant super absorbent resin is characterized by comprising the following steps: pretreatment of coal mine waste residue. The coal mine waste residue is first washed with 10% hydrochloric acid, then washed with acetone for three times, then washed with ethanol, and finally washed with distilled water. The waste residue is crushed in a 1% hydrochloric acid solution for 24 hours, and then the suspension is repeatedly washed with deionized water and dried for standby use.

[0009] Before solution polymerization, 1-10 parts of acrylic acid or methacrylic acid in the linear monomer are neutralized by 60-80% in a wide-mouth bottle with potassium hydroxide. Then, 1-10 parts of other linear monomers, 1-5 parts of salt-resistant functional monomers, and 0.02-0.20 parts of cross-linking monomers are added to the wide-mouth bottle and mixed evenly for 10 minutes, and then 0.3-1.0 parts of treated coal mine waste slag are added thereto, and then mixed evenly at 50°C for ten minutes, and the temperature is raised to 70°C and 0.05-0.15 parts of initiator are added to initiate polymerization, so that the metal ions in the coal mine waste slag participate in the polymerization cross-linking reaction to form a uniform gel product. After the reaction continues for 3 hours, the gel product is washed, dried and ground in a 60°C oven to obtain an organic-inorganic hybrid salt-resistant super absorbent resin.

[0010] After the reaction, the organic-inorganic hybrid salt-resistant superabsorbent resin was washed three times with anhydrous ethanol to remove unreacted monomers and their moisture, and placed in an oven at 60° C. until completely dried.

[0011] The beneficial effect of the present invention is that, by adding coal mine waste slag into the reaction system in the polymerization stage, the metal ions in the waste slag are effectively cross-linked and polymerized with the organic components to prepare an organic-inorganic hybrid water-absorbing resin, rather than simply using a blending method, the water retention stability, salt resistance and water absorption effect of the resin are fully improved, and the comprehensive performance is significantly improved compared with simple blending, and the deionized water absorption rate can reach 2234.52 g / g, and the 0.9% salt water absorption rate can reach 171.28 g / g. The water-absorbing resin modified by hybridization of coal mine waste slag involved in the present invention has a high water absorption rate and excellent salt resistance. Due to the introduction of waste slag inorganic materials, the cost will also be reduced accordingly. The present invention adds coal mine waste slag and organic components to cross-link and polymerize in the resin polymerization stage, improves the polymerization network of the resin, and improves the salt resistance and swelling characteristics of the water-absorbing resin. The method of pre-treating coal mine waste slag in the present invention fully cleans and crushes the coal mine waste slag so that it can be better used as a modified component of the water-absorbing resin, and the problem of utilizing specific coal mine waste slag is solved by pre-treating the coal mine waste slag. The invention fully solves the problem of high-efficiency treatment and utilization of specific coal mine waste residues, and at the same time greatly reduces the production cost of water-absorbing resin. The invention adopts potash to neutralize acrylic acid, thereby improving its biocompatibility in subsequent soil improvement. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 This is an electron microscope image of the water-absorbing resin prepared in Comparative Example 1. Figure 2 This is an electron microscope image of the water-absorbing resin prepared in Example 1. DETAILED DESCRIPTION

[0013] Example 1: Preparation of organic-inorganic hybrid salt-resistant super absorbent resin: The above-mentioned specific coal mine slag was ultrasonically cleaned with 10% hydrochloric acid, then ultrasonically cleaned three times with acetone, then ultrasonically cleaned with anhydrous ethanol, and finally ultrasonically cleaned with distilled water. Finally, it was crushed in a 1% hydrochloric acid solution for 24 hours, and then placed in an oven for drying and collection.

[0014] 3.27 g potassium hydroxide was added to 10 g water, and 6 g acrylic acid was added after ultrasonic oscillation to dissolve. 1 g of 2-acrylamide-2-methylpropanesulfonic acid was weighed and dissolved in 5 g water, and 1 g of acrylamide was weighed and dissolved in 5 g water, and ultrasonic oscillation was performed until completely dissolved. The solutions were added to the wide-mouth bottle in sequence, the temperature was raised to 50°C, and 0.03 g of N,N-methylenebisacrylamide and 0.7 g of coal mine waste slag powder were added to the reaction system. After the reaction was stable for 20 min, the temperature was raised to 70°C, 0.12 g of ammonium persulfate was dissolved in 5 g water, and ammonium persulfate was added dropwise to the mixed solution.

[0015] After reacting for 3 hours, the product was repeatedly washed three times with ethanol to remove unreacted monomers and water, and placed in a 60°C oven until completely dried to obtain an organic-inorganic hybrid salt-resistant superabsorbent resin.

[0016] When the room temperature is 25℃, weigh 0.2g of sample, pour all the sample into the tea bag, soak it in a beaker filled with deionized water or 0.9% sodium chloride salt water for 30min, take out the tea bag filled with sample, hang it with a clip, drip liquid for 10min in a static state, weigh the mass m1 of the tea bag filled with sample, use a tea bag without sample to measure the blank value at the same time, weigh the mass of the blank test tea bag, and record the mass as m2, calculate the water absorption rate according to the following formula: Water absorption rate = (m1-m2) / 0.2

[0017] Example 2: The similarities between this example and Example 1 are not repeated here, except that 3.27 g of potassium hydroxide is added to 10 g of water, and 6 g of acrylic acid is added after dissolving by ultrasonic oscillation. 1 g of N-vinyl pyrrolidone is weighed and dissolved in 5 g of water, and 1 g of acrylamide is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 ° C, and 0.03 g of N,N-methylenebisacrylamide and 0.9 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.12 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0018] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0019] Example 3: The similarities between this example and Example 1 are not repeated here, except that 3.27 g of potassium hydroxide is added to 10 g of water, and 6 g of acrylic acid is added after ultrasonic oscillation to dissolve. Weigh 1 g of 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g of water, weigh 1 g of acrylamide and dissolve it in 5 g of water, and weigh 1 g of methacrylic acid and ultrasonic oscillate it until it is completely dissolved. The solutions are added to the wide-mouth bottle in turn, the temperature is raised to 50 ° C, and 0.03 g of N,N-methylenebisacrylamide and 0.9 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.12 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0020] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0021] Example 4: The similarities between this example and Example 1 are not repeated here, except that 3.03 g of potassium hydroxide is added to 10 g of water, and 6 g of acrylic acid is added after ultrasonic oscillation dissolution. Weigh 1 g of N-vinyl pyrrolidone and dissolve it in 5 g of water, weigh 2 g of acrylamide and dissolve it in 5 g of water, and ultrasonic oscillate until completely dissolved. The solution is added to a wide-mouth bottle in sequence, heated in a water bath at 50 ° C, and after the reaction is stable for 20 min, 0.01 g of N,N-methylenebisacrylamide, 0.01 g of pentaerythritol triacrylate, 0.01 g of pentaerythritol acrylate and 0.6 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.12 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0022] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0023] Example 5: The similarities between this example and Example 1 are not repeated here, except that 3.5 g of potassium hydroxide is added to 10 g of water, and 6 g of acrylic acid is added after dissolving by ultrasonic oscillation. 2 g of 2-acrylamide-2-methylpropanesulfonic acid is weighed and dissolved in 5 g of water, 1 g of acrylamide is weighed and dissolved in 5 g of water, and 1 g of methacrylic acid is weighed and ultrasonically oscillated until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50°C, and 0.03 g of N,N-methylenebisacrylamide and 0.9 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70°C, 0.12 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0024] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0025] Example 6: The similarities between this example and Example 1 are not repeated here, except that 2.18 g of potassium hydroxide is added to 10 g of water, and 4 g of acrylic acid is added after dissolving by ultrasonic oscillation. 1 g of 2-acrylamide-2-methylpropanesulfonic acid is weighed and dissolved in 5 g of water, 2 g of acrylamide is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 ° C, and 0.02 g of N,N-methylenebisacrylamide and 0.9 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.08 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0026] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0027] Example 7: The similarities between this example and Example 1 are not repeated here, except that 4.36 g of potassium hydroxide is added to 10 g of water, and 8 g of acrylic acid is added after dissolving by ultrasonic oscillation. 2 g of 2-acrylamide-2-methylpropanesulfonic acid is weighed and dissolved in 5 g of water, and 2 g of acrylamide is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 ° C, and 0.04 g of N,N-methylenebisacrylamide and 0.9 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.12 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution.

[0028] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0029] Example 8: The similarities between this example and Example 1 are not repeated here, except that 4.36 g of potassium hydroxide is added to 10 g of water, and 8 g of acrylic acid is added after dissolving by ultrasonic oscillation. 1 g of MMA is weighed and dissolved in 5 g of water, 2 g of acrylamide is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50°C, 0.04 g of N,N-methylenebisacrylamide and 0.9 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 minutes, the temperature is raised to 70°C, 0.14 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution.

[0030] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0031] Example 9: The similarities between this example and Example 1 are not repeated here, except that 4.36 g of potassium hydroxide is added to 10 g of water, and 8 g of acrylic acid is added after being dissolved by ultrasonic oscillation. Weigh 1 g of N-vinyl pyrrolidone and dissolve it in 5 g of water, weigh 2 g of acrylamide and dissolve it in 5 g of water, weigh 1 g of 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g of water and ultrasonically oscillate it until it is completely dissolved. The solutions are added to the wide-mouth bottle in sequence, the temperature is raised to 50 ° C, and 0.04 g of N,N-methylenebisacrylamide and 0.9 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.14 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0032] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0033] Example 10: The similarities between this example and Example 1 are not repeated here, except that 2.18 g of potassium hydroxide is added to 10 g of water, and 4 g of acrylic acid is added after dissolving by ultrasonic oscillation. 1 g of N-vinyl pyrrolidone is weighed and dissolved in 5 g of water, and 1 g of acrylamide is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 °C, and 0.03 g of N,N-methylenebisacrylamide and 0.5 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 °C, 0.12 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution.

[0034] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0035] Example 11: The similarities between this example and Example 1 are not repeated here, except that 2.18 g of potassium hydroxide is added to 10 g of water, and 4 g of acrylic acid is added after dissolving by ultrasonic oscillation. 1 g of N-vinyl pyrrolidone is weighed and dissolved in 5 g of water, 2 g of MMA is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 °C, 0.01 g of N,N-methylenebisacrylamide, 0.01 g of pentaerythritol triacrylate, and 0.5 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 °C, 0.08 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0036] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0037] Example 12: The similarities between this example and Example 1 are not repeated here, except that 2.18 g of potassium hydroxide is added to 10 g of water, and 4 g of acrylic acid is added after dissolving by ultrasonic oscillation. 1 g of 2-acrylamide-2-methylpropanesulfonic acid is weighed and dissolved in 5 g of water, and 1 g of MMA is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 ° C, and 0.02 g of N,N-methylenebisacrylamide and 0.5 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.08 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0038] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0039] Example 13: The similarities between this example and Example 1 are not repeated here, except that 3.27 g of potassium hydroxide is added to 10 g of water, and 6 g of acrylic acid is added after dissolving by ultrasonic oscillation. 1 g of 2-acrylamide-2-methylpropanesulfonic acid is weighed and dissolved in 5 g of water, and 2 g of MMA is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 ° C, and 0.03 g of N,N-methylenebisacrylamide and 0.6 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.1 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0040] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0041] Example 14: The similarities between this example and Example 1 are not repeated here, except that 3.27 g of potassium hydroxide is added to 10 g of water, and 6 g of acrylic acid is added after dissolving by ultrasonic oscillation. 2 g of 2-acrylamide-2-methylpropanesulfonic acid is weighed and dissolved in 5 g of water, and 1 g of acrylamide is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 ° C, and 0.03 g of N,N-methylenebisacrylamide and 0.6 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.1 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0042] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0043] Example 15: The similarities between this example and Example 1 are not repeated here, except that 3.27 g of potassium hydroxide is added to 10 g of water, and 6 g of acrylic acid is added after ultrasonic oscillation to dissolve. 2 g of 2-acrylamide-2-methylpropanesulfonic acid is weighed and dissolved in 5 g of water, 1 g of MMA is weighed and dissolved in 5 g of water, and ultrasonic oscillation is performed until completely dissolved. The solutions are added to a wide-mouth bottle in sequence, the temperature is raised to 50 ° C, 0.02 g of N,N-methylenebisacrylamide, 0.01 g of pentaerythritol tetraacrylate and 0.5 g of coal mine waste slag powder are added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70 ° C, 0.1 g of ammonium persulfate is dissolved in 5 g of water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above.

[0044] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0045] Comparative Example 1: Preparation of a highly absorbent resin modified by non-coal mine waste residue, 3.27 g potassium hydroxide was added to 10 g water, and 6 g acrylic acid was added after ultrasonic oscillation and dissolution. 1 g 2-acrylamide-2-methylpropanesulfonic acid was weighed and dissolved in 5 g water, 1 g acrylamide was weighed and dissolved in 5 g water, and ultrasonic oscillation was performed until completely dissolved. The solution was added to a wide-mouth bottle in sequence, heated in a water bath at 50 ° C, and 0.03 g N,N-methylenebisacrylamide was added to the reaction system. After the reaction was stable for 20 min, the temperature was raised to 70 ° C, 0.12 g ammonium persulfate was weighed and dissolved in 5 g water, and ammonium persulfate was added dropwise to the mixed solution. The product was cleaned and treated as described above. The product obtained at this time is a highly absorbent resin modified by non-coal mine waste residue.

[0046] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0047] Comparative Example 2: 3.27 g potassium hydroxide was added to 10 g water, and 6 g acrylic acid was added after ultrasonic oscillation dissolution. Weigh 2 g 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g water, weigh 1 g acrylamide and dissolve it in 5 g water, weigh 1 g methacrylic acid and dissolve it in 5 g water, and ultrasonic oscillate until completely dissolved. The solution was added to the wide-mouth bottle in turn, heated in a water bath at 50 ° C, and 0.03 g of N, N-methylenebisacrylamide was added to the reaction system. The temperature was raised to 70 ° C, 0.12 g of ammonium persulfate was weighed and dissolved in 5 g water, and ammonium persulfate was added dropwise to the mixed solution. The product was cleaned and treated as described above. The product obtained at this time is a highly absorbent resin without coal mine waste slag modified hybrid. The water absorption rate was tested according to the experimental method described in Example 1.

[0048] Comparative Example 3: 8.18 g potassium hydroxide is added to 10 g water, and 15 g acrylic acid is added after ultrasonic oscillation dissolution. Weigh 2 g 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g water, weigh 2 g acrylamide and dissolve it in 5 g water, and ultrasonic oscillate until completely dissolved. The solution is added to the wide-mouth bottle in sequence, heated to 50 ° C in a water bath, and 0.05 g of N, N-methylenebisacrylamide is added to the reaction system. The temperature is raised to 70 ° C, 0.2 g of ammonium persulfate is weighed and dissolved in 5 g water, and ammonium persulfate is added dropwise to the mixed solution. The product is cleaned and treated as described above. The product obtained at this time is an absorbent resin with excess acrylic acid and no coal mine waste residue. The water absorption rate test is carried out according to the experimental method described in Example 1.

[0049] Comparative Example 4: The coal mine waste slag used is as described in the above waste slag pretreatment method. 3.27 g potassium hydroxide is added to 10 g water, and 6 g acrylic acid is added after ultrasonic oscillation dissolution. Weigh 1 g 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g water, weigh 1 g acrylamide and dissolve it in 5 g water, and ultrasonic oscillate until completely dissolved. The solution is added to a wide-mouth bottle in turn, heated in a water bath at 50 ° C, and 0.02 g N,N-methylenebisacrylamide and 3 g coal mine waste slag powder are added to the reaction system. The temperature is raised to 70 ° C, 0.1 g ammonium persulfate is weighed and dissolved in 5 g water, and ammonium persulfate is added dropwise to the mixed solution.

[0050] The product is cleaned and treated as described above. The product obtained at this time is a water-absorbent resin containing excessive coal mine waste slag hybrid modification. The water absorption rate test is carried out according to the experimental method described in Example 1.

[0051] Comparative Example 5: The coal mine waste slag used is as described in the above waste slag pretreatment method. 3.27 g potassium hydroxide is added to 10 g water, and 6 g acrylic acid is added after ultrasonic oscillation dissolution. Weigh 1 g 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g water, weigh 1 g acrylamide and dissolve it in 5 g water, and ultrasonic oscillate until completely dissolved. The solution is added to a wide-mouth bottle in turn, heated in a water bath at 50 ° C, and 0.2 g N,N-methylenebisacrylamide and 0.7 g coal mine waste slag powder are added to the reaction system. The temperature is raised to 70 ° C, 0.1 g ammonium persulfate is weighed and dissolved in 5 g water, and ammonium persulfate is added dropwise to the mixed solution.

[0052] The product is cleaned and treated as described above. The product obtained at this time is a waste residue hybrid water-absorbent resin containing excessive N,N-methylenebisacrylamide. The water absorption rate test is carried out according to the experimental method described in Example 1.

[0053] Comparative Example 6: The coal mine waste slag used is as described in the above waste slag pretreatment method. 3.27 g potassium hydroxide is added to 10 g water, and 6 g acrylic acid is added after ultrasonic oscillation dissolution. Weigh 1 g 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g water, weigh 1 g acrylamide and dissolve it in 5 g water, and ultrasonic oscillate until completely dissolved. The solution is added to a wide-mouth bottle in turn, heated in a water bath at 50°C, and 0.03 g N,N-methylenebisacrylamide and 0.7 g coal mine waste slag powder are added to the reaction system. The temperature is raised to 70°C, 1 g ammonium persulfate is weighed and dissolved in 5 g water, and ammonium persulfate is added dropwise to the mixed solution.

[0054] The product is cleaned and treated as described above. The product obtained at this time is the waste residue hybrid water-absorbent resin using excess ammonium persulfate. The water absorption rate test is carried out according to the experimental method described in Example 1.

[0055] Comparative Example 7: The coal mine waste slag used is as described in the above waste slag pretreatment method. 3.27 g potassium hydroxide is added to 10 g water, and 6 g acrylic acid is added after ultrasonic oscillation to dissolve. Weigh 1 g 2-acrylamide-2-methylpropanesulfonic acid and dissolve it in 5 g water, weigh 1 g acrylamide and dissolve it in 5 g water, and ultrasonic oscillate until completely dissolved. The solutions are added to the wide-mouth bottle in turn, the temperature is raised to 50°C, and 0.03 g N,N-methylenebisacrylamide is added to the reaction system. After the reaction is stable for 20 min, the temperature is raised to 70°C, 0.12 g ammonium persulfate is dissolved in 5 g water, and ammonium persulfate is added dropwise to the mixed solution. The product cleaning and treatment methods are as described above. The above product is blended with 0.7 g of treated coal mine waste slag as a water-absorbing resin.

[0056] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0057] Comparative Example 8: A water-absorbent resin prepared according to the method of Example 1 of 201310694751.3. The water absorption rate test was performed according to the experimental method described in Example 1.

[0058] Comparative Example 9: A water-absorbent resin prepared according to the method of 201911222950.8 Example 2. The water absorption rate test was performed according to the experimental method described in Example 1.

[0059] Comparative Example 10

[0060] Commercially available water-absorbing resin neutralized with sodium alkali and acrylic acid.

[0061] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0062] Comparative Example 11

[0063] Commercially available water-absorbing resins for neutralizing acrylic acid with potassium alkali.

[0064] The water absorption rate test was carried out according to the experimental method described in Example 1.

[0065] The absorption properties of the water-absorbent resins prepared in the above Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 and Comparative Examples 1, 2, 3, 4, 5, 6, 7, 8, 9 and the water absorption properties of the commercially available super absorbent resin Comparative Examples 10 and 11 are compared as shown in Table 1.

[0066] Table 1 Comparison of the absorption performance of water-absorbent resins

[0067]

[0068]

[0069] Table 1 shows the deionized water absorption rate of the water-absorbing resin prepared in each embodiment. It can be seen that the water absorption rate of the water-absorbing resin prepared by adding coal mine waste slag and not adding waste slag components is quite different, among which the water absorption rate of Example 1 is the best. Compared with Comparative Example 1, it is found that the resin without adding coal mine waste slag has poor water absorption. According to the scanning electron microscope analysis, the high water-absorbing resin without adding waste slag presents a dense structure at a scale of 50μm, and there are basically no cracks on the whole. Many other homogeneous water-absorbing resins studied all present this state, which is the result of the cross-linking of polymer chains by the cross-linking agent. In contrast, the spatial structure produced by the waste slag introduced during the polymerization process significantly improves the polymer network structure, presents an irregular porous structure, and there are a large number of pits and micropores, which promotes the diffusion of water into the water-absorbing resin network, and the overall structure is looser. At the same time, the uniform and loose pore structure can provide a large amount of water storage space, which is conducive to the rapid infiltration of water molecules into the resin, improves the water absorption rate, and greatly improves the salt resistance. Compared with the two commercially available products, the super absorbent resin modified by coal mine waste slag hybridization has greatly improved both in terms of deionized water absorption and salt water resistance. For the absorbent resin with added waste slag, when the amount of waste slag is 0.7-0.9 parts, the deionized water absorption rate is generally above 2000g / g, and the absorption rate of 0.9% salt water is above 140g / g. The effect is better when the amount of waste slag exceeds 0.9 parts and is less than 0.7 parts.

[0070] In addition, the absorption rates of deionized water and 0.9% salt water in Comparative Examples 1, 2, and 3 without slag crosslinking and Comparative Example 4 with more than 20% slag are generally reduced. At the same time, for Comparative Examples 5 and 6 with excessive crosslinking agent N,N-methylenebisacrylamide and excessive ammonium persulfate, the absorption rates of the two types of water are also greatly reduced. For Comparative Example 7 in which the organic component and the waste slag are directly mixed together by blending, the water absorption rate is lower than that of Comparative Examples 1 and 2 without waste slag. For Comparative Examples 8 and 9 of the water-absorbent resin prepared by the disclosed patent preparation method, the absorption rate of deionized water and 0.9% salt water is worse than that of the water-absorbent resin modified by waste slag. In addition, commercially available water-absorbent resins such as Comparative Examples 10 and 11 have poor performance in absorbing deionized water and 0.9% salt water.

Claims

1. An organic-inorganic hybrid salt-tolerant superabsorbent resin, characterized in that The invention comprises the following components in parts by weight: 1-10 parts of linear monomers, 1-5 parts of salt-resistant functional monomers, 0.02-0.04 parts of cross-linking monomers, 0.05-0.15 parts of initiators, and 0.3-1.0 parts of coal mine waste slag, wherein the metal contents of mercury in the coal mine waste slag are 0.003 µg / g, lead is 30.8 µg / g, cadmium is 3.30 µg / g, barium is 887 µg / g, and Sr is 390 µg / g; the linear monomers are two or three of methacrylic acid, acrylic acid, and acrylamide; the salt-resistant functional monomers are 2-acrylamide-2-methylpropane sulfonic acid and / or N-vinyl pyrrolidone; the cross-linking monomers are one or more of N,N-methylenebisacrylamide, pentaerythritol triacrylate, and pentaerythritol tetraacrylate; and the initiator is ammonium persulfate.

2. A method for preparing an organic-inorganic hybrid salt-tolerant superabsorbent resin, characterized in that The method comprises the following steps: the content of metals in the coal mine waste slag is 0.003 µg / g of mercury, 30.8 µg / g of lead, 3.30 µg / g of cadmium, 887 µg / g of barium, and 390 µg / g of Sr; the coal mine waste slag pretreatment method is: the coal mine waste slag is first washed with 10% hydrochloric acid, then washed with acetone three times, then washed with ethanol, and finally washed with distilled water; the coal mine waste slag is crushed in a 1% hydrochloric acid solution for 24 hours, and then the suspension is repeatedly washed with deionized water, and dried for standby use; Before solution polymerization, 1-10 parts of acrylic acid or methacrylic acid in the linear monomer are neutralized by 60-80% in a wide-mouth bottle using potassium hydroxide; then 1-10 parts of other linear monomers, 1-5 parts of salt-resistant functional monomers, and 0.02-0.20 parts of cross-linking monomers are added to the wide-mouth bottle and mixed evenly for 10 minutes, then 0.3-1.0 parts of treated coal mine waste slag are added thereto, and then mixed evenly at 50°C for ten minutes, the temperature is raised to 70°C, and 0.05-0.15 parts of initiator are added to initiate polymerization; the metal ions in the coal mine waste slag are involved in the polymerization cross-linking reaction to form a uniform gel product; after the reaction continues for 3 hours, the gel product is washed, and dried and ground in an oven at 60°C to obtain an organic-inorganic hybrid salt-resistant superabsorbent resin.

3. The method for preparing the organic-inorganic hybrid salt-tolerant superabsorbent resin according to claim 2, characterized in that After the reaction, the organic-inorganic hybrid salt-resistant superabsorbent resin was washed three times with anhydrous ethanol to remove unreacted monomers and their moisture, and placed in an oven at 60° C. until completely dried.