A kind of polyether modified low hydrogen silicone oil and preparation method thereof
By introducing amide and phosphate-based structures into polyether modified silicone oil, cloud point is reduced and stability and surfactivity is improved, the problems of single performance and poor stability in the prior art are solved, and multifunctional and extensive Used polyether modified low hydrogen-containing silicone oil.
Patent Information
- Application Number
- CN202310393079.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-13
AI Technical Summary
The existing polyether modified silicone oil has single performance and poor stability, and cannot take into account both defoaming, interfacial activity and low cloud point, and its application range is limited.
The conventional polyether modified silicone oil was modified by amide-containing modified polyether and polyether phosphate structure, and the allyl alcohol polyoxyethylene polyoxypropylene ether and N-BOC-3-amino-3-methyl Butyric acid reaction, combined with low hydrogen-containing silicone oil and allyl polyoxyethylene polyoxypropylene methyl ether, and then reacted with phosphorus oxychloride to produce polyether-modified low hydrogen-containing silicone oil.
It reduces cloud point, improves the stability, lubricity, defoaming, interface activity and antistatic properties of the product, expands the scope of application, and is suitable for low-temperature defoaming and multi-functional use.
Smart Images

Figure CN116554480B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicone oil, and in particular to a polyether-modified low-hydrogen silicone oil and a preparation method thereof. Background Art
[0002] Silicone oil is a very safe liquid, harmless to the body, with good stability and a pH value of about 7. The stable structure of polysiloxane determines its stable chemical properties. It accounts for a large proportion of silicon-containing polymers, has good functions, a wide variety of models, few restrictions on use, and is used in many industrial fields. By changing the degree of polymerization of polysiloxane or the type of organic group or copolymerizing polysiloxane with other organic matter, different types of silicone oil can be obtained. The structure determines the properties. The performance of these modified silicone oils is better. According to the requirements of the application environment, corresponding silicone oils can be obtained, such as heat-resistant silicone oil, silicone oil with excellent surface properties, silicone oil with stable chemical properties, water-soluble silicone oil, high specific heat capacity silicone oil, etc. Modified silicone oil can also be further made into silicone grease, silicone paste, release agent, anti-adhesive agent, defoaming agent, polishing agent, etc. through compounding and other means.
[0003] At present, various modified silicone oils are widely used in fabric softening and simulation finishing, shampoo and daily chemicals due to their good hydrophilicity, strong hygroscopicity, softening, antistatic, wetting and other functions.
[0004] Among modified silicone oils, polyether-modified silicone oil is the most widely used and produced type at present. It mainly refers to a type of oily polymer in which the side chain or main chain of linear dimethyl silicone oil is connected to the polyether segment through a chemical bond. In the molecular structure of this silicone oil, the polyether segment contains a highly polar oxygen atom connected to carbon, which can form a hydrogen bond with water and is hydrophilic and soluble in water. The silicone oil bond energy in the polysiloxane segment is high, relatively stable, neither hydrophilic nor lipophilic, and the inactive hydrocarbon group on the main chain of the silicone oil is also not hydrophilic. Therefore, when these two segments are connected together, the surface tension of the aqueous solution can be effectively reduced. It is a type of surfactant with excellent performance.
[0005] However, most polyether-modified silicone oils in the prior art are modified with a single polyether. The polyethers have the same structure, relatively simple performance, poor stability, and limited application range, and cannot take into account multiple functions at the same time. In addition, when polyether-modified silicone oil is used as a defoamer, the foam system temperature must be higher than its cloud point temperature to have a defoaming effect. However, the cloud point temperature of polyether-modified silicone oils in the prior art is relatively high, and it cannot play a defoaming role under low temperature conditions, and the application environment is limited.
[0006] Therefore, there is an urgent need for a polyether-modified silicone oil having multiple polyether structures, which can simultaneously take into account defoaming properties, interfacial activity and stability and has a low cloud point. Summary of the invention
[0007] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide a polyether-modified low-hydrogen silicone oil having a variety of polyether structures, which can simultaneously take into account defoaming properties, interfacial activity and stability and has a low cloud point and a wide range of applications, and a preparation method thereof.
[0008] Technical solution:
[0009] A polyether-modified low-hydrogen silicone oil, wherein the polyether-modified low-hydrogen silicone oil has a structure as shown in the following formula A:
[0010]
[0011] Among them, m=120-160, x=8-12, y=4-8, a=8-12, b=7-10, c=8-12, d=7-10, and m, x, y, a, b, c, d are integers.
[0012] The polyether-modified low-hydrogen silicone oil provided by the present invention uses an amide-containing modified polyether and a polyether phosphate structure to modify conventional polyether-modified silicone oil, thereby reducing the cloud point of conventional polyether-modified silicone oil, allowing the product to have multiple properties and better stability at the same time, and having a wider range of applications.
[0013] The preparation method of the above-mentioned polyether-modified low-hydrogen silicone oil comprises the following steps:
[0014] (1) preparing a modified polyether by reacting allyl alcohol polyoxyethylene polyoxypropylene ether with N-BOC-3-amino-3-methylbutyric acid;
[0015] (2) preparing modified silicone oil by low hydrogen silicone oil, allyl polyoxyethylene polyoxypropylene methyl ether and modified polyether;
[0016] (3) The polyether-modified low-hydrogen silicone oil is prepared by reacting modified silicone oil with phosphorus oxychloride.
[0017] Further, the structure of the allyl alcohol polyoxyethylene polyoxypropylene ether is, wherein a=8-12, b=7-10;
[0018] The structure of the allyl polyoxyethylene polyoxypropylene methyl ether is, wherein c=8-12, d=7-10.
[0019] Furthermore, the specific method of step (1) is: in a reactor, add allyl alcohol polyoxyethylene polyoxypropylene ether, inhibitor and catalyst-1, heat to 70-90°C, stir evenly and then add N-BOC-3-amino-3-methylbutyric acid, heat to 120-140°C, react for 6-8 hours, adjust the product to neutral, wash, dry and filter to obtain the modified polyether.
[0020] The reaction process is:
[0021]
[0022] The polyether-modified low-hydrogen silicone oil provided by the present invention is grafted with a modified polyether. Since the modified polyether contains a plurality of branched alkyl groups, the surface tension of the aqueous solution can be greatly reduced, and the product can have better lubricity, defoaming and anti-sticking properties; at the same time, the amide group contained in the modified polyether structure can improve the compatibility of the product with the skin, reduce irritation, and is conducive to biodegradation and reduces environmental pollution.
[0023] Furthermore, the polymerization inhibitor is selected from one of hydroquinone, p-hydroxyanisole or 2,6-di-tert-butyl-p-cresol; and the catalyst-1 is p-toluenesulfonic acid.
[0024] Furthermore, the mass ratio of the allyl alcohol polyoxyethylene polyoxypropylene ether to N-BOC-3-amino-3-methylbutyric acid is 10:1.6-2.2.
[0025] Furthermore, the specific method of step (2) is: in a reactor, add a solvent, low hydrogen silicone oil, allyl polyoxyethylene polyoxypropylene methyl ether and modified polyether, heat to 90-110°C, add catalyst-2, stir the reaction for 6-8 hours and then remove the solvent to obtain a yellow transparent liquid, which is the modified silicone oil.
[0026] The reaction process is:
[0027] in,
[0028] n=x+y.
[0029] Furthermore, the hydrogen content of the low hydrogen silicone oil is 0.15%-0.2%; the catalyst-2 is a platinum catalyst; the effective platinum content in the catalyst-2 is 1.0×10 of the total mass of the reactants. -5 -5.0×l0 -5 .
[0030] Furthermore, the mass ratio of the low hydrogen silicone oil, allyl polyoxyethylene polyoxypropylene methyl ether and modified polyether is 12:(8-12):(5-10).
[0031] Furthermore, the specific method of step (3) is: adding phosphorus oxychloride into the reactor, adding modified silicone oil dropwise under stirring, maintaining the temperature at 10-15°C, stirring for 10-20 minutes, heating to 40-50°C, reacting for 6-8 hours, and obtaining a polyether-modified low-hydrogen silicone oil having a structure as shown in the above formula A.
[0032] The polyether-modified low-hydrogen silicone oil provided by the present invention has a polyether phosphate structure obtained by the reaction of allyl alcohol polyether and phosphorus oxychloride, so that the product has excellent interfacial activity, antistatic property, thermal stability and good compatibility, and has the characteristics of nonionic and anionic surfactants, which plays an important role in reducing interfacial tension, preventing calcium ion scaling and corrosion inhibition.
[0033] Furthermore, the mass ratio of the phosphorus oxychloride to the modified silicone oil is 3-5:500.
[0034] Beneficial effects:
[0035] (1) The polyether-modified low-hydrogen silicone oil provided by the present invention is grafted with a modified polyether. Since the modified polyether contains multiple branched alkyl groups, the surface tension of the aqueous solution can be greatly reduced, and the product can have better lubricity, defoaming and anti-sticking properties; at the same time, the amide group contained in the modified polyether structure can improve the compatibility of the product with the skin, reduce irritation, and is conducive to biodegradation and reduce environmental pollution.
[0036] (2) The polyether-modified low-hydrogen silicone oil provided by the present invention has a polyether phosphate structure grafted thereon obtained by reacting allyl alcohol polyether with phosphorus oxychloride, which can make the product have excellent interfacial activity, antistatic properties, thermal stability and good compatibility, and at the same time has the characteristics of nonionic and anionic surfactants, which plays an important role in reducing interfacial tension, preventing calcium ion scaling and corrosion inhibition.
[0037] (3) The polyether-modified low-hydrogen silicone oil provided by the present invention can reduce the cloud point of conventional polyether-modified silicone oil by using modified polyether containing amide groups and polyether phosphate structures to modify conventional polyether-modified silicone oil, so that the product can have multiple properties and better stability at the same time, and has a wider range of applications. DETAILED DESCRIPTION
[0038] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0039] The platinum catalyst was 965005 purchased from Bailingwei Technology Co., Ltd. and diluted to a mass fraction of 4.0×10 -3; Allyl alcohol polyoxyethylene polyoxypropylene ether was purchased from Wuhan Rongcan Biotechnology Co., Ltd.; allyl polyoxyethylene polyoxypropylene methyl ether was purchased from Hangzhou Diweilai Trading Co., Ltd.; low hydrogen silicone oil was purchased from Huangshan Keberi New Material Technology Co., Ltd.; N-BOC-3-amino-3-methylbutyric acid was BD89210 purchased from Shanghai Bide Pharmaceutical Technology Co., Ltd.; phosphorus oxychloride was purchased from Nanjing Xiezun Pharmaceutical Technology Co., Ltd.; the remaining reagents and equipment were conventional reagents and equipment in this technical field.
[0040] Example 1
[0041] (1) Add 10g of allyl alcohol polyoxyethylene polyoxypropylene ether, 0.1g of hydroquinone, and 0.1g of p-toluenesulfonic acid to a three-necked flask equipped with a thermometer, a condenser, and a stirrer, and heat to 70°C. After stirring evenly, add 2g of N-BOC-3-amino-3-methylbutyric acid, heat to 120°C, and react for 6 hours. When the temperature of the reaction system drops to 90°C, perform vacuum distillation to remove the generated water. Hydroquinone, p-toluenesulfonic acid, and unreacted N-BOC-3-amino-3-methylbutyric acid precipitate as colorless crystals and are separated to obtain a brown-yellow transparent liquid. The crude product is adjusted to neutral with sodium carbonate solution, then washed with saturated NaCl solution, the organic layer is separated, dried and filtered with anhydrous calcium chloride, and further dehydrated by vacuum distillation to obtain pure modified polyether;
[0042] (2) In a three-necked flask equipped with a stirrer, a reflux condenser and a thermometer, 50 ml of ethylene glycol dimethyl ether, 12 g of low hydrogen silicone oil, 8 g of allyl polyoxyethylene polyoxypropylene methyl ether and 5 g of modified polyether were added, heated to 90° C., 0.1 ml of platinum catalyst was added at a constant temperature, stirred and reacted for 6 hours, and the ethylene glycol dimethyl ether solvent was removed from the system by reduced pressure distillation to obtain a light yellow transparent liquid, which was the modified silicone oil;
[0043] (3) Add 0.5 g of phosphorus oxychloride to a four-necked flask equipped with a thermometer, a stirrer and other hydrogen chloride absorption devices, add 50 g of modified silicone oil dropwise while stirring, maintain the temperature at 10° C., stir for 10 minutes, then raise the temperature to 40° C. and react for 6 hours to obtain the polyether-modified low-hydrogen silicone oil.
[0044] Example 2
[0045] The method is basically the same as Example 1, except that in step (1), hydroquinone is replaced by an equal amount of p-hydroxyanisole; and in step (2), the masses of allyl polyoxyethylene polyoxypropylene methyl ether and modified polyether are changed to 12 g and 7 g, respectively.
[0046] Example 3
[0047] The method is basically the same as Example 1, except that in step (1), hydroquinone is replaced by an equal amount of 2,6-di-tert-butyl-p-cresol; and in step (2), the masses of allyl polyoxyethylene polyoxypropylene methyl ether and modified polyether are changed to 10 g and 10 g, respectively.
[0048] Comparative Example 1
[0049] Commercially available polyether modified silicone oil (204 water-soluble silicone oil purchased from Qingdao Kunrong New Materials Co., Ltd.).
[0050] Comparative Example 2
[0051] The process is basically the same as Example 1, except that steps (1) and (3) are not performed, and the modified polyether in step (2) is replaced by an equal amount of allyl polyoxyethylene polyoxypropylene methyl ether.
[0052] Comparative Example 3
[0053] The process is basically the same as Example 1, except that step (1) is not performed and the modified polyether in step (2) is replaced by an equal amount of allyl alcohol polyoxyethylene polyoxypropylene ether.
[0054] Comparative Example 4
[0055] The process is basically the same as Example 1, except that step (3) is not performed.
[0056] Comparative Example 5
[0057] The process is basically the same as Example 1, except that in step (2), the masses of allyl polyoxyethylene polyoxypropylene methyl ether and modified polyether are changed to 5 g and 12 g, respectively.
[0058] Performance Testing
[0059] Surface tension measurement: The products of Examples 1-3 and Comparative Examples 1-5 were prepared into aqueous solutions with a mass fraction of 5%, and the surface tension of the aqueous solutions was measured by a contact angle meter.
[0060] Turbidity point determination: According to the method for determining the turbidity point of ethylene oxide type and ethylene oxide-propylene oxide block polymerization type nonionic surfactants in GB / T5559-2010, the turbidity points of the products of Examples 1-3 and Comparative Examples 1-5 were determined.
[0061] The test results are shown in the following table:
[0062]
[0063]
[0064] According to the test results of Examples 1-3 and Comparative Example 1, the polyether-modified low-hydrogen silicone oil provided by the present invention has stronger surface activity and a lower cloud point, and can be suitable for defoaming purposes in low-temperature environments.
[0065] According to the test results of Examples 1-3 and Comparative Examples 2-4, the grafted polyether, amide group, phosphate group, branched alkyl group and other structures in the polyether-modified low-hydrogen silicone oil provided by the present invention can effectively enhance the surface activity of the silicone oil and effectively reduce the cloud point.
[0066] According to the test results of Examples 1-3 and Comparative Examples 2-3, the polyether-modified low-hydrogen silicone oil provided by the present invention is grafted with different amide groups, phosphate groups and multi-branched alkyl groups, which can effectively reduce the cloud point of the silicone oil and improve its surface activity.
[0067] According to the test results of Examples 1-3 and Comparative Examples 3-4, the grafted polyether phosphate structure in the polyether-modified low-hydrogen silicone oil provided by the present invention can effectively improve the interfacial activity of the product, reduce the interfacial tension, and provide surface activity.
[0068] According to the test results of Examples 1-3 and Comparative Example 5, the polyether-modified low-hydrogen silicone oil provided by the present invention can be prepared by a limited ratio to obtain silicone oil having both strong surface activity and a low cloud point.
[0069] Preparation of emulsion: Add hydrophobic white carbon black and the products of Examples 1-3 and Comparative Examples 1-5 in a mass ratio of 1:10 into a round-bottom flask, stir in an oil bath and heat to 150°C, react at a constant temperature for 4 hours, then reduce to 85°C, add emulsifiers Span80 and Tween80, and thickener glyceryl monostearate, the mass ratio of Span80, Tween80 and glyceryl monostearate is 2.5:1.2:1. Stir at room temperature with a shear dispersion emulsifier at a speed of 10000r / min for about 2 minutes, add a certain amount of water during high-speed stirring, and obtain a white silicone emulsion defoamer product with an active ingredient mass fraction of 20%.
[0070] Thermal stability test: Measure 2g of white silicone emulsion defoamer sample, put it into a sealable test tube, and place it in an environment of 110℃, 120℃, 140℃ and 160℃ for 30 minutes. Take it out and observe whether there is oil floating after the temperature drops, and record the temperature at which oil floating begins to occur.
[0071] Storage stability test: Take 50 mL of white silicone emulsion defoamer sample, let it stand at room temperature for three weeks, and observe whether it is stratified.
[0072] Defoaming test:
[0073] Preparation of standard foaming solution: Weigh 5 g of nonylphenol polyoxyethylene ether and 5 g of sodium dodecylbenzene sulfonate and dissolve them in 990 mL of water. Mix and stir until a uniform transparent liquid is obtained.
[0074] Use a measuring cylinder to measure 50 mL of the standard foaming solution, add 0.1 g of white silicone emulsion defoamer, keep the temperature at 50°C in a water bath, cover the bottle with a stopper, and shake the measuring cylinder vertically up and down 30 times at a frequency of 2 times per second and an amplitude of (30-35) cm. Let it stand and start using a stopwatch to record the time it takes for the foam to disappear and the liquid surface to appear, in seconds.
[0075] The test results are shown in the following table:
[0076] Thermal stability (oil drift temperature) Storage stability Defoaming time(s) Example 1 160℃ no 5 Example 2 160℃ no 4 Example 3 160℃ no 5 Comparative Example 1 120℃ no 10 Comparative Example 2 120℃ no 8 Comparative Example 3 140℃ no 9 Comparative Example 4 120℃ no 6 Comparative Example 5 160℃ no 6
[0077] According to the test results of Examples 1-3 and Comparative Example 1, the polyether-modified low-hydrogen silicone oil provided by the present invention has stronger thermal stability and stronger defoaming ability.
[0078] According to the test results of Examples 1-3 and Comparative Examples 2-4, the grafted polyether, amide, phosphate and other structures in the polyether-modified low-hydrogen silicone oil provided by the present invention can effectively enhance the stability of the silicone oil, and the grafted multi-branched alkyl can effectively improve the defoaming ability of the silicone oil.
[0079] According to the test results of Examples 1-3 and Comparative Examples 2-3, the polyether-modified low-hydrogen silicone oil provided by the present invention is grafted with different amide groups, phosphate groups and multi-branched alkyl groups, which can effectively improve the stability of the silicone oil.
[0080] According to the test results of Examples 1-3 and Comparative Example 4, the grafted polyether phosphate structure in the polyether-modified low-hydrogen silicone oil provided by the present invention can effectively improve the thermal stability of the product.
[0081] According to the test results of Examples 1-3 and Comparative Example 5, the polyether-modified low-hydrogen silicone oil provided by the present invention can be prepared in a limited ratio to obtain silicone oil with good stability and defoaming ability.
[0082] According to the test results of the examples and comparative examples in the two tables, the polyether-modified low-hydrogen silicone oil provided by the present invention can take into account defoaming properties, interfacial activity and stability at the same time and has a low cloud point.
[0083] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyether-modified low-hydrogen silicone oil, characterized in that: The polyether-modified low-hydrogen silicone oil has a structure shown in the following formula A: ; Among them, m=120-160, x=8-12, y=4-8, a=8-12, b=7-10, c=8-12, d=7-10, and m, x, y, a, b, c, d are integers.
2. A method for preparing the polyether-modified low-hydrogen silicone oil according to claim 1, characterized in that: The following steps are involved: (1) The modified polyether is prepared by reacting allyl alcohol polyoxyethylene polyoxypropylene ether with N-BOC-3-amino-3-methylbutyric acid; (2) preparing modified silicone oil by reacting low hydrogen silicone oil, allyl polyoxyethylene polyoxypropylene ether and modified polyether; (3) The polyether-modified low-hydrogen silicone oil is prepared by reacting modified silicone oil with phosphorus oxychloride.
3. The method for preparing a polyether-modified low-hydrogen silicone oil according to claim 2, characterized in that: The specific method of step (1) is as follows: in a reactor, add allyl alcohol polyoxyethylene polyoxypropylene ether, inhibitor and catalyst-1, heat to 70-90°C, stir evenly and then add N-BOC-3-amino-3-methylbutyric acid, heat to 120-140°C, react for 6-8 hours, adjust the product to neutral, wash, dry and filter to obtain the modified polyether.
4. The method for preparing the polyether-modified low-hydrogen silicone oil according to claim 3, characterized in that: The polymerization inhibitor is selected from one of hydroquinone, p-hydroxyanisole or 2,6-di-tert-butyl-p-cresol; and the catalyst-1 is p-toluenesulfonic acid.
5. The method for preparing the polyether-modified low-hydrogen silicone oil according to claim 3, characterized in that: The mass ratio of the allyl alcohol polyoxyethylene polyoxypropylene ether to N-BOC-3-amino-3-methylbutyric acid is 10:1.6-2.
2.
6. The method for preparing the polyether-modified low-hydrogen silicone oil according to claim 2, characterized in that: The specific method of step (2) is as follows: in a reactor, a solvent, low hydrogen silicone oil, allyl polyoxyethylene polyoxypropylene ether and modified polyether are added, heated to 90-110° C., catalyst-2 is added, and the reaction is stirred for 6-8 hours and then the solvent is removed to obtain a yellow transparent liquid, which is the modified silicone oil.
7. The method for preparing the polyether-modified low-hydrogen silicone oil according to claim 6, characterized in that: The hydrogen content of the low hydrogen silicone oil is 0.15%-0.2%; the catalyst-2 is a platinum catalyst; the effective platinum content in the catalyst-2 is 1.0×10 of the total mass of the reactants. -5 -5.0×l0 -5 .
8. The method for preparing the polyether-modified low-hydrogen silicone oil according to claim 6, characterized in that: The mass ratio of the low hydrogen silicone oil, allyl polyoxyethylene polyoxypropylene ether and modified polyether is 12: (8-12): (5-10).
9. The method for preparing a polyether-modified low-hydrogen silicone oil according to claim 2, characterized in that: The specific method of step (3) is as follows: add phosphorus oxychloride into the reactor, add modified silicone oil dropwise under stirring, maintain the temperature at 10-15° C., stir for 10-20 minutes, heat to 40-50° C., react for 6-8 hours, and the polyether modified low hydrogen silicone oil can be obtained.
10. The method for preparing the polyether-modified low-hydrogen silicone oil according to claim 9, characterized in that: The mass ratio of the phosphorus oxychloride to the modified silicone oil is 3-5:500.