Long-life multi-layer composite thermal barrier coating and preparation method thereof

By preparing YSZ toughened layers and GZ-YSZ composite ceramic layers using multilayer composite structures and suspension plasma spraying technology, the problem of easy failure of thermal barrier coatings at high temperatures was solved, and thermal barrier coatings with high fracture toughness and long life were achieved.

CN118910534APending Publication Date: 2024-11-08INNER MONGOLIA UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410990627.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing thermal barrier coating materials are prone to sintering and damage at high temperatures, leading to premature coating failure. Furthermore, traditional YSZ materials have low fracture toughness, making it difficult to meet the requirements for long life and high-temperature stability.

Method used

A multi-layer composite structure is adopted, including a metal bonding layer, a toughening layer and a composite ceramic layer. The YSZ toughening layer and the GZ-YSZ composite ceramic layer are prepared by suspension plasma spraying technology. The spraying parameters and suspension composition are controlled to form columnar structures and vertical cracks, thereby improving the bonding strength and toughness.

Benefits of technology

It enhances the fracture toughness and bonding strength of the coating, extends the thermal cycling life, and enables stable operation at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910534A_ABST
    Figure CN118910534A_ABST
Patent Text Reader

Abstract

The invention discloses a long-service-life multi-layer composite thermal barrier coating and a preparation method thereof. The thermal barrier coating sequentially comprises three layers of structures from a base body to the outside, the inner layer is a metal bonding layer, the middle layer is a toughening layer, and the top layer is a composite ceramic layer. The toughening layer and the composite ceramic layer have columnar and vertical crack structures. The columnar YSZ toughening layer prepared through SPS spraying is adopted, the toughness of the toughening layer can be effectively improved, the fracture toughness of the composite ceramic layer is improved by adding different contents of YSZ into GZ, the difference of the thermal expansion coefficients of the top layer and the middle layer is effectively reduced, and it is guaranteed that the thermal barrier coating stably serves at the high temperature for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, in particular to a long-life multi-layer composite thermal barrier coating and a preparation method thereof. Background Art

[0002] Thermal barrier coatings (TBCs) are widely used on the surfaces of metal hot end components of gas turbine engines, mainly to reduce heat transfer and protect the metal substrate. The main performance criteria of industrial gas turbine TBCs are excellent thermal shock life and thermal cycle fatigue life. Traditional TBCs are composed of a ceramic surface layer, a metal bonding layer, and a thermally grown oxide (TGO) layer.

[0003] Since the 1980s, 7-8wt.% yttria partially stabilized zirconia (6-8YSZ) has been the material of choice for ceramic layers. YSZ has excellent thermomechanical properties, such as low thermal conductivity (2.1 W·m -1 ·K -1 ), coefficient of thermal expansion (CTE) (~11.7×10 -6 K -1 ) and metal bonding layer (~15×10 -6 K -1 ) with high fracture toughness (~2.5-3.5MPa·m 1 / 2 ), has good thermal cycling performance, etc., but YSZ material will undergo significant sintering and destructive volume phase change above 1200℃, resulting in premature failure of the coating.

[0004] Gd2Zr2O7 (GZ) is a new type of thermal barrier coating material with high melting point, low thermal conductivity, high phase stability (its order-disorder transition at high temperature will not have an adverse effect on thermal cycle life), excellent resistance to CMAS erosion, and high thermal expansion coefficient (9-11×10 -6 K -1 ), however, GZ has low fracture toughness and easily reacts with alumina (TGO) to form porous GdAlO3. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to provide a long-life multilayer composite thermal barrier coating with high fracture toughness, low elastic modulus and long thermal cycle life and a preparation method thereof.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A long-life multi-layer composite thermal barrier coating, which includes three layers from the substrate to the outside, the inner layer is a metal bonding layer, the middle layer is a toughening layer, and the top layer is a composite ceramic layer; the toughening layer and the composite ceramic layer have columnar and vertical crack structures. The metal bonding layer uses CoCrNiAlY metal powder.

[0008] In the above-mentioned long-life multi-layer composite thermal barrier coating, the metal bonding layer is obtained by a deposition method on a base alloy; the toughening layer is a YSZ toughening layer prepared by suspension plasma spraying SPS technology; and the composite ceramic layer is a gadolinium zirconate GZ-YSZ composite ceramic layer prepared by suspension plasma spraying SPS technology.

[0009] In the above-mentioned long-life multi-layer composite thermal barrier coating, the thickness of the metal bonding layer is 100-150 μm, the thickness of the toughening layer is 50-150 μm, and the thickness of the composite ceramic layer is 250-350 μm.

[0010] The toughening layer with nano- and submicron structures was prepared by SPS spraying in the middle layer, and the composite ceramic layer with column gaps and vertical cracks was prepared by SPS spraying in the outermost layer. On the one hand, the toughening layer and the composite ceramic layer have good wettability because the SPS coating is composed of nano- and submicron structures. On the other hand, the mutual diffusion of elements between the two layers under high temperature conditions may also promote bonding, making the bonding strength between the toughening layer and the composite ceramic layer higher. At the same time, the sintering of the composite ceramic layer during the thermal cycle causes the coating to shrink, which eventually causes the expansion of the column gap. The presence of column gaps and vertical cracks improves the strain tolerance of the coating.

[0011] The present application controls the size of the sprayed droplets, thereby using SPS to obtain a toughening layer and a composite ceramic layer with a columnar structure.

[0012] The above-mentioned long-life multi-layer composite thermal barrier coating, in the suspension system for preparing the toughening layer, uses ammonium polyacrylate as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the ball milling time of the system is controlled to be 1-3h, alcohol is used as a suspension medium, the solid content of the system is 10-20wt%, the pH value of the system is controlled to be 7-9, the viscosity of the system is 0.3-0.6mPa·s, and the surface tension of the system is 21-26mN / m;

[0013] In the preparation of the composite ceramic layer suspension system, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the ball milling time of the system is controlled to be 1-3h, the solid content of the system is 10-20wt%, the YSZ accounts for 0-50% of the solid mass content, the gadolinium zirconate GZ accounts for 50%-100% of the solid mass content, the pH value of the system is controlled to be 7-9, the viscosity of the system is 0.3-0.6mPa·s, and the surface tension of the system is 21-26mN / m.

[0014] The present application controls the system viscosity and surface tension of the suspension, thereby controlling the particle size D50 of the spray droplets within the range of 1-2 μm, thereby obtaining a stable columnar structure and vertical cracks.

[0015] A method for preparing a long-life multi-layer composite thermal barrier coating comprises the following steps:

[0016] (A) depositing a metal bonding layer on a nickel-based alloy substrate;

[0017] (B) spraying a YSZ toughening layer on the metal bonding layer using a suspension plasma spraying SPS technology to obtain a toughening layer;

[0018] (C) A layer of gadolinium zirconate GZ-YSZ composite ceramic layer is sprayed on the toughening layer using suspension plasma spraying SPS technology to obtain a composite ceramic layer.

[0019] In the above method for preparing a long-life multi-layer composite thermal barrier coating, in step (A), the thickness of the metal bonding layer is 100-150 μm.

[0020] In the above-mentioned method for preparing a long-life multi-layer composite thermal barrier coating, in step (B), alcohol is used as a suspension medium, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content of the system is 10-20wt%, the pH value of the system is controlled to be 7-9, the ball milling time of the system is controlled to be 1-3h, the viscosity of the system is 0.3-0.6mPa·s, the surface tension of the system is 21-26mN / m, and the thickness of the layered toughening layer is 50-150μm. The pH value is controlled at 7-9, which can change the dissociation degree of the dispersant, and then change the adsorption state and adsorption amount of the dispersant on the particle surface. Ammonium polyacrylate is used as an anionic dispersant. Therefore, the alkalinity of the system is conducive to the dispersion stability of the system.

[0021] The above-mentioned method for preparing a long-life multi-layer composite thermal barrier coating, in step (C), in the suspension used for the composite ceramic layer, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content is 10-20wt%, the YSZ accounts for 0-50% of the solid mass content; the gadolinium zirconate GZ accounts for 50%-100% of the solid mass content, the system pH value is controlled to 7-9, the ball milling time of the system is controlled to 1-3h, the system viscosity is controlled to 0.3-0.6mPa·s, and the system surface tension is 21-26mN / m; the thickness of the composite ceramic layer is 250-350μm.

[0022] The solid content of the suspension is controlled at 10-20%. The solid content control is mainly to improve the balance between deposition efficiency and smooth liquid delivery during thermal spraying. An increase in solid content will lead to an increase in the viscosity of the suspension system, which is not conducive to liquid delivery during thermal spraying.

[0023] In the above-mentioned method for preparing a long-life multi-layer composite thermal barrier coating, in step (C), in step (B) and step (C), the suspension plasma spraying SPS technical process parameters are: spraying distance 60-80mm, gun moving speed 600-800mm / s, stepping 1-1.5mm / step, and deposition temperature 130-180℃.

[0024] The above-mentioned method for preparing a long-life multi-layer composite thermal barrier coating comprises the following steps:

[0025] (A) depositing a metal bonding layer on a nickel-based alloy substrate; the thickness of the metal bonding layer is 100-150 μm;

[0026] (B) spraying a YSZ toughening layer on the metal bonding layer by using a suspension plasma spraying SPS technology to obtain a toughening layer; in the suspension system for the toughening layer, alcohol is used as a suspension medium, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content of the system is 10-20wt%, the pH value of the system is controlled to be 7-9, the ball milling time of the system is controlled to be 1-3h, the viscosity of the system is 0.3-0.6mPa·s, and the surface tension of the system is 21-26mN / m; the thickness of the toughening layer is 50-150μm;

[0027] (C) spraying a gadolinium zirconate GZ-YSZ composite ceramic layer on the toughening layer by using a suspension plasma spraying SPS technology to obtain a composite ceramic layer; in the suspension used to prepare the composite ceramic layer, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content is 10-20wt%, the YSZ accounts for 0-50% of the solid mass content, and the gadolinium zirconate GZ accounts for 50%-100% of the solid mass content, the system pH value is controlled to 7-9, the system ball milling time is controlled to 1-3h, the system viscosity is controlled to 0.3-0.6mPa·s, and the system surface tension is controlled to 21-26mN / m; the thickness of the composite ceramic layer is 250-350μm;

[0028] In step (B) and step (C), the suspension plasma spraying SPS technical process parameters are: spraying distance 60-80mm, gun moving speed 600-800mm / s, stepping 1-1.5mm / step, and deposition temperature 130-180°C. Controlling the deposition temperature at 130-180°C can ensure that the density of vertical cracks is within the range of 3.4-4.7 / mm. If there are too many vertical cracks, the ability to resist stress will decrease. If the density of vertical cracks is too small, the stress release is insufficient, which is not conducive to the toughness and cycle life of the composite ceramic.

[0029] The technical solution of the present invention achieves the following beneficial technical effects:

[0030] The present application adopts suspension plasma spraying (SPS) to prepare a yttria partially stabilized zirconia (YSZ) toughening layer and a composite ceramic layer of gadolinium zirconate GZ-YSZ (GZ-YSZ) with different composition ratios. The toughening layer and the composite ceramic layer prepared by the present invention both have a typical columnar structure and vertical cracks, the interface between the toughening layer and the composite ceramic layer is well bonded, and the coating fracture toughness of the gadolinium zirconate GZ-YSZ composite ceramic layer toughened by YSZ is increased. Therefore, the thermal barrier coating designed and prepared by the present invention has the advantages of strong bonding, high temperature resistance, and long life.

[0031] The columnar YSZ toughening layer prepared by SPS spraying is used in this application to effectively improve the toughness of the toughening layer. Different contents of YSZ are added to GZ to improve the fracture toughness of the composite ceramic layer, effectively reduce the difference in thermal expansion coefficients between the top layer and the middle layer, and ensure that the thermal barrier coating can serve stably for a long time at high temperatures.

[0032] The toughening layer and composite ceramic layer prepared in the present application are both in the form of columnar structures. The interface between the composite ceramic layer and the YSZ toughening layer is well bonded without horizontal cracks. On the one hand, because the SPS coatings of the toughening layer and the composite ceramic layer are composed of nano and submicron structures, the wettability between the particles is good. On the other hand, the mutual diffusion of elements between the two layers under high temperature conditions may also promote bonding, making the bonding strength between the toughening layer and the composite ceramic layer higher.

[0033] In thermal spraying, atmospheric plasma spraying mainly forms a layered structure, solution plasma spraying obtains interlayer gaps + vertical crack structures, electron beam physical vapor deposition can obtain a columnar crystal structure, and plasma physical vapor deposition can obtain a layered / feathered / columnar structure. Although electron beam physical vapor deposition and plasma physical vapor deposition can obtain columnar structures, the preparation costs of both are relatively high.

[0034] The present application uses a suspension plasma spraying method, controls the suspension system and the spraying process, thereby obtaining a toughening layer and a composite ceramic layer with a columnar structure and vertical cracks. The present application controls the viscosity and surface tension of the system by adding a dispersant ammonium polyacrylate during the suspension preparation process and controlling the ball milling time of the dispersion system, and then controls the spraying process so that the size of the sprayed droplets can be controlled, thereby obtaining a toughening layer and a composite ceramic layer with a columnar structure.

[0035] Controlling the deposition temperature at 130-180°C can ensure that the density of vertical cracks is within the range of 3.4-4.7 / mm. If there are too many vertical cracks, the stress resistance will decrease. If the density of vertical cracks is too small, the stress release will be insufficient, which is not conducive to the toughness and cycle life of the composite ceramic.

[0036] In the suspension system, when alcohol is used as a solvent, the surface tension is reduced, the droplets obtained by atomization are small, and a columnar structure + vertical crack structure can be stably obtained. When water or water + alcohol is used as a solvent, a layered structure will appear. The layered structure has the risk of peeling, which is not conducive to the stability of thermal cycle performance. The solid content in the suspension system will affect the deposition efficiency and coating structure of the coating. When the solid content is less than 10%, only a layered structure can be obtained. When the solid content is higher than 20%, transverse cracks appear on the columnar structure. The layered structure or transverse cracks will affect the toughness and cycle life of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematic diagram of different GZ-YSZ contents in the long-life multi-layer composite thermal barrier coating structure of the present invention;

[0038] Figure 2 Microscopic morphology of thermal barrier coating with composite ceramic layer containing 50GZ-50YSZ;

[0039] Figure 3 Microscopic morphology of thermal barrier coating with composite ceramic layer containing 80GZ-20YSZ;

[0040] Figure 4 Microscopic morphology of thermal barrier coating with composite ceramic layer containing 100GZ;

[0041] Figure 5a This is the microscopic morphology of the coating when the solvent of the toughening layer suspension is water; Figure 5b This is the microscopic morphology of the coating when the solvent of the toughening layer suspension is 50% water + 50% alcohol; Figure 5c This is the microscopic morphology of the coating when the solvent of the toughening layer suspension is alcohol. DETAILED DESCRIPTION

[0042] Embodiment 1:

[0043] This example aims to explore the stability of the suspension, using 50wt% deionized water and 50wt% alcohol as the solvent of the suspension, 0.5wt% ammonium polyacrylate as the dispersant, adding YSZ powder, controlling the solid content of the system to 10wt%, the ball milling time to 1.5h, and the pH of the system to 10. The stability results show that the viscosity of the system is 3.11mPa·s, the surface tension is 30.4mN / m, the sedimentation height is 6.2ml, and the median diameter is 0.877μm.

[0044] Embodiment 2:

[0045] This example aims to explore the stability of the suspension, using 100wt% alcohol as the solvent of the suspension, 0.5wt% ammonium polyacrylate as the dispersant, adding YSZ powder, controlling the solid content of the system to 15wt%, the ball milling time to 2h, and the pH value of the system to 8. The suspension stability results show that the viscosity of the system is 0.45mPa·s, the surface tension is 24.6mN / m, the sedimentation height is 0.3ml, and the median diameter is 1.6μm.

[0046] Embodiment 3:

[0047] Schematic diagram of coating structure Figure 1 As shown, the present invention aims to provide a long-life multi-layer composite thermal barrier coating and a preparation method thereof, comprising the following steps:

[0048] Step 1: deposit a 150 μm thick metal bonding layer on a nickel-based high-temperature alloy substrate.

[0049] Step 2: Prepare a 50 μm thick YSZ toughening layer on the metal bonding layer by plasma spraying of a suspension. The specific spraying process is as follows: a spraying distance of 60 mm, a gun moving speed of 700 mm / s, a stepping distance of 1 mm / step, and specific parameters of the suspension: the suspension medium is 100% alcohol, the solid content of the YSZ powder is 20 wt.%, the pH value of the suspension is 8, and the ball milling is 2 h. At this time, the viscosity of the suspension is 0.45 mPa·s, the surface tension is 24.6 mN / m, and D50=1.634 μm.

[0050] Step 3: Continue to use suspension plasma spraying to form a 50GZ-50YSZ composite coating with a thickness of 250 μm on the YSZ toughening layer. The solid content of the suspension is 10 wt %. The specific spraying process is as follows: a coating distance of 60 mm, a gun moving speed of 700 mm / s, and a stepping distance of 1 mm / step.

[0051] The composite coating structure prepared is as follows Figure 2As shown, the different ceramic layers are well bonded, the porosity of the composite ceramic layer is 21%, the column density is 6.34 / mm, the vertical crack density is 4.45 / mm, the elastic modulus is 181.53Gpa, and the fracture toughness is 1.77MPa·m 1 / 2 In the furnace cycle test at 1100°C, the cycle life of the structural coating reached 542 times.

[0052] Embodiment 4:

[0053] The difference between this embodiment and embodiment 3 is that the suspension used for spraying in step 3 is 60GZ-40YSZ, and the spraying process is the same.

[0054] The prepared composite coating has good bonding between different ceramic layers, with a porosity of 21%, a column density of 6.57 / mm, and a vertical crack density of 4.21 / mm. In a furnace cycle test at 1100°C, the cycle life of the structural coating reached 621 times.

[0055] Embodiment 5:

[0056] The difference between this embodiment and embodiment 3 is that the suspension used for spraying in step 3 is 70GZ-30YSZ, and the spraying process is the same.

[0057] The prepared composite coating has good bonding between different ceramic layers, with a porosity of 19%, a column density of 6.88 / mm, and a vertical crack density of 3.58 / mm. In a furnace cycle test at 1100°C, the cycle life of the structural coating reached 825 times.

[0058] Embodiment 6:

[0059] The difference between this embodiment and embodiment 3 is that the suspension used for spraying in step 3 is 80GZ-20YSZ, and the spraying process is the same.

[0060] The composite coating structure prepared is as follows Figure 3 As shown, the different ceramic layers are well bonded, the porosity of the composite ceramic layer is 17%, the column density is 6.95 / mm, the vertical crack density is 3.48 / mm, the elastic modulus is 124.19 Gpa, and the fracture toughness is 1.92 MPa·m 1 / 2 In the furnace cycle test at 1100°C, the cycle life of the structural coating reached 1025 times.

[0061] Embodiment 7:

[0062] The difference between this embodiment and embodiment 3 is that the suspension used for spraying in step 3 is 90GZ-10YSZ, and the spraying process is the same.

[0063] The prepared composite coating has good bonding between different ceramic layers, with a porosity of 21%, a column density of 7.21 / mm, and a vertical crack density of 3.56 / mm. In a furnace cycle test at 1100°C, the cycle life of the structural coating reached 820 times.

[0064] Embodiment 8:

[0065] The difference between this embodiment and embodiment 3 is that a YSZ coating with a thickness of 300 μm is prepared by spraying directly on the metal bonding layer.

[0066] The prepared coating has good bonding with the metal bonding layer, the porosity of the ceramic layer is 22%, the column density is 7.12 / mm, and the vertical crack density is 4.21 / mm. The cycle life of the structural coating reached 450 times in the furnace cycle test at 1100℃.

[0067] Embodiment 9:

[0068] The difference between this embodiment and embodiment 6 is that the thickness of the prepared 80GZ-20YSZ composite ceramic layer is 300 μm.

[0069] The prepared composite coating has good bonding between different ceramic layers, with a porosity of 18%, a column density of 7.01 / mm, and a vertical crack density of 3.52 / mm. In a furnace cycle test at 1100°C, the cycle life of the structural coating reached 921 times.

[0070] Embodiment 10:

[0071] The difference between this embodiment and embodiment 6 is that the thickness of the prepared 80GZ-20YSZ composite ceramic layer is 350 μm.

[0072] The prepared composite coating has good bonding between different ceramic layers, with a porosity of 17%, a column density of 6.87 / mm, and a vertical crack density of 3.49 / mm. In a furnace cycle test at 1100°C, the cycle life of the structural coating reached 842 times.

[0073] Embodiment 11:

[0074] The difference between this embodiment and embodiment 6 is that the solid content of the suspension used is 15wt%, the suspension composition is 80GZ-20YSZ, and the specific spraying process is spraying distance 70mm, gun moving speed 700mm / s, and stepping 1mm / step.

[0075] The prepared composite coating has good bonding between different ceramic layers, with a porosity of 19%, a column density of 6.63 / mm, and a vertical crack density of 4.01 / mm. In a furnace cycle test at 1100°C, the cycle life of the structural coating reached 786 times.

[0076] Example 12

[0077] The difference between this embodiment and embodiment 6 is that the solid content of the suspension used is 20wt%, the suspension composition is 80GZ-20YSZ, and the specific spraying process is spraying distance 80mm, gun moving speed 700mm / s, and stepping 1mm / step.

[0078] The prepared composite coating has good bonding between different ceramic layers, with a porosity of 21%, a column density of 6.98 / mm, and a vertical crack density of 4.32 / mm. In a furnace cycle test at 1100°C, the cycle life of the structural coating reached 752 times.

[0079] Embodiment 13

[0080] The difference between this embodiment and embodiment 3 is that the suspension used for spraying in step 3 is 100GZ, the spraying process is the same, and the structure is as follows Figure 4 shown.

[0081] The prepared composite coating has good bonding between different ceramic layers. The porosity of the composite ceramic layer is 25%, the column density is 6.64 / mm, the vertical crack density is 4.71 / mm, the elastic modulus is 190.51Gpa, and the fracture toughness is 1.33MPa·m 1 / 2 In the furnace cycle test at 1100°C, the cycle life of the structural coating reached 631 times.

[0082] Table 1 is a comparative summary of Examples 3 to 13.

[0083] Table 1

[0084]

[0085] Table 2 is a comparison table of the fracture toughness and elastic modulus of Example 3, Example 6 and Example 13.

[0086] Table 2

[0087]

[0088] Summary of Example Results:

[0089] The present invention prepares composite ceramic layers with different GZ / YSZ ratios by designing the composition of the composite ceramic layer, and introduces an intermediate layer of YSZ prepared by SPS as a toughening layer for the entire system. Such a structural design enables the target coating to serve stably for a long time in a high temperature environment.

[0090] No obvious delamination was observed at the interface between the GZ-YSZ composite ceramic layer and the YSZ toughening layer, that is, the bonding strength between the two layers was high. This good bonding is mainly due to the fact that the SPS coating is composed of nano- and submicron structures, and the wettability between the particles is good. At the same time, the mutual diffusion of elements between the two layers under high temperature conditions may also promote bonding. The column gaps and vertical crack extensions throughout the entire ceramic layer can be clearly observed in all coatings. During the thermal cycle, the sintering of the ceramic layer causes the coating to shrink, which eventually causes the expansion of the column gaps. The presence of column gaps and vertical cracks improves the strain tolerance of the coating.

[0091] It can be seen from Examples 3 and 8 that increasing the thickness of the toughening layer, increasing the porosity and column density are detrimental to the thermal cycle life and reducing the cycle life.

[0092] It can be seen from Examples 6, 9 and 10 that as the thickness of the composite ceramic layer increases, the porosity, column density and vertical crack density decrease, and the cycle life decreases.

[0093] It can be seen from Examples 6, 11 and 12 that increasing the solid content of the suspension is not conducive to extending the cycle life.

[0094] It can be seen from Example 3, Example 6, and Example 13 in Table 2 that after compounding YSZ in the GZ coating, the fracture toughness of the coating is improved and the elastic modulus is reduced. Both changes are conducive to extending the cycle life of the coating.

[0095] In addition, the solvents for the suspension were screened:

[0096] The suspension solvents were water, 50wt% water + 50wt% alcohol and 100wt% alcohol, respectively, and the solid content of the system was 10wt%. The morphology of the toughening layer coating obtained was as follows: Figure 5a-5c When the solvent is water, only a lamellar structure can be obtained, but no columnar structure. When dissolved as 50wt% water + 50wt% alcohol, a lamellar structure + vertical cracks are obtained. Only when alcohol is used as the solvent, a columnar structure + vertical crack structure is obtained.

[0097] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.

Claims

1. A long-life multi-layer composite thermal barrier coating, characterized in that: The thermal barrier coating comprises three layers from the substrate to the outside, the inner layer is a metal bonding layer, the middle layer is a toughening layer, and the top layer is a composite ceramic layer; the toughening layer and the composite ceramic layer have columnar and vertical crack structures.

2. A long-life multi-layer composite thermal barrier coating according to claim 1, characterized in that: The metal bonding layer is obtained by a deposition method on a base alloy; the toughening layer is a YSZ toughening layer prepared by a suspension plasma spraying SPS technology; and the composite ceramic layer is a gadolinium zirconate GZ-YSZ composite ceramic layer prepared by a suspension plasma spraying SPS technology.

3. A long-life multi-layer composite thermal barrier coating according to claim 2, characterized in that: The thickness of the metal bonding layer is 100-150 μm, the thickness of the toughening layer is 50-150 μm, and the thickness of the composite ceramic layer is 250-350 μm.

4. The long-life multi-layer composite thermal barrier coating according to claim 2, characterized in that: In the suspension system for preparing the toughening layer, alcohol is used as the suspension medium, ammonium polyacrylate is used as the dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content of the system is 10-20wt%, the pH value of the system is controlled to be 7-9, the ball milling time of the system is controlled to be 1-3h, the viscosity of the system is controlled to be 0.3-0.6mPa·s, and the surface tension of the system is 21-26mN / m; In the suspension system for preparing the composite ceramic layer, alcohol is used as the suspension medium, ammonium polyacrylate is used as the dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content of the system is 10-20wt%, the YSZ accounts for 0-50% of the solid mass content, the gadolinium zirconate GZ accounts for 50%-100% of the solid mass content, the pH value of the system is controlled to be 7-9, the ball milling time of the system is controlled to be 1-3h, the viscosity of the system is controlled to be 0.3-0.6mPa·s, and the surface tension of the system is controlled to be 21-26mN / m.

5. A method for preparing a long-life multi-layer composite thermal barrier coating according to any one of claims 1 to 4, characterized in that: The steps include: (A) depositing a metal bonding layer on a nickel-based alloy substrate; (B) spraying a YSZ toughening layer on the metal bonding layer using a suspension plasma spraying SPS technology to obtain a toughening layer; (C) A layer of gadolinium zirconate GZ-YSZ composite ceramic layer is sprayed on the toughening layer using suspension plasma spraying SPS technology to obtain a composite ceramic layer.

6. The method for preparing a long-life multi-layer composite thermal barrier coating according to claim 5, characterized in that: In step (A), the thickness of the metal bonding layer is 100-150 μm.

7. The method for preparing a long-life multi-layer composite thermal barrier coating according to claim 5, characterized in that: In step (B), in the suspension system for preparing the toughening layer, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, alcohol is used as a suspension medium, the solid content of the system is 10-20wt%, the pH value of the system is controlled to 7-9, the ball milling time of the system is controlled to 1-3h, the viscosity of the system is controlled to 0.3-0.6mPa·s, the surface tension of the system is 21-26mN / m, and the thickness of the toughening layer is 50-150μm.

8. The method for preparing a long-life multi-layer composite thermal barrier coating according to claim 5, characterized in that: In step (C), in the suspension for preparing the composite ceramic layer, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, alcohol is used as a suspension medium, the solid content is 10-20wt%, YSZ accounts for 0-50% of the solid mass content; gadolinium zirconate GZ accounts for 50%-100% of the solid mass content, the system pH value is controlled to 7-9, the system ball milling time is controlled to 1-3h, the system viscosity is controlled to 0.3-0.6mPa·s, and the system surface tension is controlled to 21-26mN / m; the thickness of the composite ceramic layer is 250-350μm.

9. The method for preparing a long-life multi-layer composite thermal barrier coating according to claim 5, characterized in that: In step (C), in step (B) and step (C), the suspension plasma spraying SPS technical process parameters are: spraying distance 60-80mm, gun moving speed 600-800mm / s, stepping 1-1.5mm / step, and deposition temperature is 130-180℃.

10. A method for preparing a long-life multi-layer composite thermal barrier coating according to claim 5, characterized in that: The steps include: (A) depositing a metal bonding layer on a nickel-based alloy substrate; the thickness of the metal bonding layer is 100-150 μm; (B) spraying a YSZ toughening layer on the metal bonding layer by using a suspension plasma spraying SPS technology to obtain a toughening layer; in the suspension system for the toughening layer, alcohol is used as a suspension medium, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content of the system is 10-20wt%, the pH value of the system is controlled to be 7-9, the ball milling time of the system is controlled to be 1-3h, the viscosity of the system is 0.3-0.6mPa·s, the surface tension of the system is 21-26mN / m, and the thickness of the toughening layer is 50-150μm; (C) spraying a gadolinium zirconate GZ-YSZ composite ceramic layer on the toughening layer by using a suspension plasma spraying SPS technology to obtain a composite ceramic layer; in the suspension used to prepare the composite ceramic layer, alcohol is used as a suspension medium, ammonium polyacrylate is used as a dispersant, the content of ammonium polyacrylate is 0.5wt%, the solid content is 10-20wt%, wherein YSZ accounts for 0-50% of the solid mass content, and gadolinium zirconate GZ accounts for 50%-100% of the solid mass content, the system pH value is controlled to 7-9, the system ball milling time is controlled to 1-3h, the system viscosity is controlled to 0.3-0.6mPa·s, and the system surface tension is controlled to 21-26mN / m; the thickness of the composite ceramic layer is 250-350μm; In step (B) and step (C), the suspension plasma spraying SPS technical process parameters are: spraying distance 60-80mm, gun moving speed 600-800mm / s, stepping 1-1.5mm / step, and deposition temperature 130-180°C.

Citation Information

Cited By

  • Layered hafnium silicate bonding layer with low annealing temperature as well as preparation method and application of layered hafnium silicate bonding layer

    CN122059727A

  • Abradable coating system with good abradability and method to produce it

    GB2704205A