Cationic rosin / furfural urea resin composite sizing agent and preparation method thereof
In the papermaking industry, a composite sizing agent combining uronic urea resin made by the condensation polymerization of urea and maltose and modified cationic rosin has been used to solve the problem of rosin price fluctuations, achieve cost reduction and improve the water resistance of paper.
Patent Information
- Application Number
- CN202310837460.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-07-10
AI Technical Summary
The fluctuation of rosin prices in the existing paper industry makes sizing costs difficult to control. It is necessary to develop a lower-cost, easy-to-manufacture rosin supplement to replace or reduce the dosage of rosin.
The uronic urea resin made by the condensation polymerization of urea and maltose is combined with modified cationic rosin to form a cationic rosin/uronic urea resin composite sizing agent, which is emulsified through metal ion catalysts and emulsifiers to form a stable emulsion state to replace Partly rosin.
It reduces the production cost, improves the water resistance and printing adaptability of the paper, and the urea resin itself is low-toxic, environmentally friendly, and highly stable, avoiding the impact of rosin price fluctuations.
Smart Images

Figure BDA0004329373980000051 
Figure BDA0004329373980000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of papermaking sizing agents, in particular to a composite sizing agent containing furfural urea resin and a preparation method thereof. Background Art
[0002] Rosin is a mixture of resin acid, a small amount of fatty acid, rosin anhydride and other substances. It is often used as an internal sizing agent in the papermaking field. It is mainly used to improve the water resistance of paper, prevent ink penetration, and facilitate printing. The price of rosin fluctuates due to seasonal influences, and the cost of sizing is difficult to control. Therefore, a low-cost and easy-to-manufacture rosin supplement needs to be developed to alleviate the impact of rosin price fluctuations. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a furfural urea resin composite sizing agent and a preparation method thereof which can replace or reduce the amount of rosin used. The furfural resin formed by the polycondensation of maltose and urea under the action of a catalyst can replace part of the rosin and be used in a papermaking sizing agent. A new sizing agent product can be developed, the product stability and sizing effect can be improved, and the production cost can be reduced.
[0004] The present invention is achieved by adopting the following technical solutions:
[0005] A cationic rosin / furfural urea resin composite sizing agent is composed of cationic rosin, furfural urea resin and an appropriate amount of emulsifier, wherein the furfural urea resin accounts for 4-30% of the total weight of the cationic rosin and the furfural urea resin; the cationic rosin is maleic anhydride and fumaric acid modified rosin, and the furfural urea resin is polycondensed from urea and maltose.
[0006] The cationic rosin is prepared by conventional methods in the art, for example, by the following method: 70-95 parts by weight of rosin is added into a reaction kettle, heated to 180-220° C., and then 3.5-8 parts by weight of maleic anhydride and fumaric acid are added to modify the rosin, wherein the maleic anhydride and fumaric acid are compounded in a weight ratio of 1:1.
[0007] The urea and maltose in the furfural urea resin are polycondensed in a molar ratio of (1-4): (1-2). For example, the following method is used for preparation: urea and maltose are added to a reaction kettle in proportion, stirring is started, heating is increased to 70-110° C., a metal ion catalyst is added, and the reaction time is 5-8 hours and then cooled to room temperature to obtain a reddish brown viscous furfural urea resin.
[0008] The metal ion catalyst is selected from at least one of zinc acetate, magnesium acetate, nickel acetate and copper acetate; the added mass percentage is 0.1-2%.
[0009] The cationic rosin / furfural urea resin composite sizing agent of the present invention can use an emulsifier commonly used in the art, preferably a cationic emulsifier, preferably a composite cationic emulsifier composed of a cationic quaternary ammonium salt surfactant and polyamide polyamine epichlorohydrin.
[0010] The inventors found that after the furfural urea resin is emulsified by an emulsifier, if there is no synergistic effect of cationic rosin, the product will be stratified in a short time and cannot form a stable emulsion state; when the substitution amount of the furfural urea resin reaches more than 30%, the emulsification effect will also deteriorate, the color of the rubber material will become darker, and small brown granular substances will appear during emulsification. Therefore, the optimal substitution amount of the furfural urea resin is between 4-30%.
[0011] The present invention further provides a method for preparing the above-mentioned cationic rosin / furfural urea resin composite sizing agent, comprising the following steps:
[0012] S1, urea and maltose are added to the reaction kettle in proportion, stirring is started, heating is increased to 70-110°C, metal ion catalyst is added, reaction time is 5-8h, and the temperature is cooled to room temperature to obtain furfural urea resin;
[0013] S2, adding rosin into a reaction kettle, heating to 180-220° C., and then adding maleic anhydride and fumaric acid to modify the rosin to obtain cationic rosin;
[0014] S3, cooling to 120-150° C., adding the furfural urea resin in an amount of 5-30% of the mass of the rosin, mixing evenly, adding an emulsifier in an amount of 10-30% of the mass of the rosin under high-speed stirring, the temperature is 60-95° C., stirring evenly, adding hot water for phase inversion, adjusting the solid content to 30-50%, cooling to room temperature, and obtaining a cationic rosin / furfural urea resin composite sizing agent.
[0015] Preferably, the emulsifier is a composite emulsifier of a cationic quaternary ammonium salt surfactant and polyamide polyamine epichlorohydrin, wherein the cationic quaternary ammonium salt surfactant accounts for 20-50% of the total weight of the composite emulsifier.
[0016] Preferably, in step S3, the stirring speed when adding hot water for phase inversion is controlled at 1500-2000 rpm / min.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1) The present invention introduces furfural urea resin to replace part of the cationic rosin. The furfural resin formed by the polycondensation of maltose and urea has the advantages of low toxicity, environmental protection and low cost, and has more hydroxyl groups. When added to rosin, it is more conducive to the phase inversion emulsification of rosin, and the obtained emulsion is more stable.
[0019] 2) The use of furfural urea resin to prepare rosin glue not only reacts the carboxyl group of rosin with the hydroxyl group of the fiber, but also the emulsion can penetrate into the fiber after adding to the pulp, and undergo dehydration condensation with the hydroxyl group of the fiber, which reduces the sliding property between the fibers after the paper is soaked in water, and not only improves the water resistance of the paper, but also produces a certain wet strength effect. The excellent properties of furfural urea resin and rosin are comprehensively utilized, and the prepared sizing agent emulsion is stable and non-stratified, and effectively improves the water resistance and printing adaptability of the paper after sizing.
[0020] 3) The raw material of furfural urea resin is cheap and easy to obtain, and its price is not restricted by season, which greatly reduces the cost of rubber. DETAILED DESCRIPTION
[0021] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only used as examples, but are not used to limit the scope of the present invention. Those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalent solutions, and other technical solutions that do not deviate from the spirit and scope of the present invention.
[0022] The instruments or raw materials in the present invention that do not indicate the manufacturer are all conventional commercial instruments or raw materials. Maleic anhydride and fumaric acid are compounded in a mass ratio of 1:1, and the composite cationic emulsifier is a composite emulsifier of cationic quaternary ammonium salt surfactant and polyamide polyamine epichlorohydrin, wherein the cationic quaternary ammonium salt surfactant accounts for 20% of the total weight of the composite emulsifier.
[0023] Unless otherwise mentioned, the detection indicators involved in the embodiments of the present invention are detected by conventional detection methods in the art.
[0024] Example 1
[0025] Weigh 60 g of urea and 342 g of maltose into a dry reactor, start stirring, heat to 70° C., add 8 g of zinc acetate, react for 5 h, and cool the temperature to room temperature to obtain a reddish brown viscous furfural urea resin.
[0026] 70g of rosin was added into a reaction kettle, heated to 180°C, and then 3.5g of maleic anhydride and fumaric acid were added to modify the rosin. After modification, the temperature was lowered to 150°C, and 3.5g of the furfural urea resin synthesized in the first step was added. After mixing evenly, 21g of a composite cationic emulsifier was added under high-speed stirring. The emulsifier was first heated to 60°C, stirred evenly, and then hot water was added for phase inversion. The rotation speed was controlled to 1500rmp / min during the phase inversion, and the solid content was adjusted to 30%. The mixture was cooled to room temperature to obtain a cationic rosin / furfural urea resin composite sizing agent.
[0027] Example 2
[0028] Weigh 120 g of urea and 1000 g of maltose into a dry reactor, start stirring, heat to 90° C., add 1.12 g of magnesium acetate, react for 8 h, and cool the temperature to room temperature to obtain a reddish-brown viscous furfural urea resin.
[0029] 95g of rosin was added into a reaction kettle, heated to 180°C, and then 7.6g of maleic anhydride and fumaric acid were added to modify the rosin. After modification, the temperature was lowered to 120°C, and 19g of the furfural urea resin synthesized in the first step was added. After mixing evenly, 28.5g of a composite cationic emulsifier was added under high-speed stirring. The emulsifier was first heated to 60°C, stirred evenly, and then hot water was added for phase inversion. The rotation speed was controlled to 1800rmp / min during the phase inversion, and the solid content was adjusted to 40%. The mixture was cooled to room temperature to obtain a cationic rosin / furfural urea resin composite sizing agent.
[0030] Example 3
[0031] Weigh 90 g of urea and 1368 g of maltose into a dry reactor, start stirring, heat to 110° C., add 1.4 g of nickel acetate, react for 6 h, and cool the temperature to room temperature to obtain a reddish-brown viscous furfural urea resin.
[0032] 80g of rosin was added into a reaction kettle, heated to 220°C, and then 4g of maleic anhydride and fumaric acid were added to modify the rosin. After modification, the temperature was lowered to 130°C, and 24g of the furfural urea resin synthesized in the first step was added. After mixing evenly, 16g of a composite cationic emulsifier was added under high-speed stirring. The emulsifier was first heated to 95°C, stirred evenly, and then hot water was added for phase inversion. During the phase inversion, the speed was controlled to 2000rmp / min, the solid content was adjusted to 40%, and the mixture was cooled to room temperature to obtain a cationic rosin / furfural urea resin composite sizing agent.
[0033] Example 4
[0034] Weigh 60 g of urea and 1200 g of maltose into a dry reactor, start stirring, heat to 100° C., add 1.2 g of copper acetate, react for 7 h, and cool the temperature to room temperature to obtain a reddish-brown viscous furfural urea resin.
[0035] 80g of rosin was added into a reaction kettle, heated to 200°C, and then 4g of maleic anhydride and fumaric acid were added to modify the rosin. After modification, the temperature was lowered to 140°C, and 16g of the furfural urea resin synthesized in the first step was added. After mixing evenly, 8g of a composite cationic emulsifier was added under high-speed stirring. The emulsifier was first heated to 80°C, stirred evenly, and then hot water was added for phase inversion. During the phase inversion, the speed was controlled to be 2000rmp / min, the solid content was adjusted to 50%, and the mixture was cooled to room temperature to obtain a cationic rosin / furfural urea resin composite sizing agent.
[0036] Comparative Example
[0037] 80g of rosin is added into a reaction kettle, heated to 200°C, and then 4g of maleic anhydride and fumaric acid are added to modify the rosin. After modification, the temperature is lowered to 140°C, and 8g of a composite cationic emulsifier is added under high-speed stirring. The emulsifier is first heated to 80°C, stirred evenly, and then hot water is added for phase inversion. During the phase inversion, the speed is controlled to be 2000rmp / min, the solid content is adjusted to 40%, and cooled to room temperature to obtain a cationic rosin glue.
[0038] Application Examples
[0039] The sizing agents of Examples 1-4 and the comparative example were applied to paper pulp for internal sizing, with an addition amount of 9 kg / t paper.
[0040] The specific process is as follows:
[0041] Designed papermaking weight 100g / m 2
[0042] Process: pulp 85% + aluminum sulfate + rosin glue + talc 15% + CPAM (200ppm)
[0043] Rosin glue addition amount 9kg / t paper (wet / dry, each sample is added at 35% solid content.)
[0044] According to the above process, the pH value of the blank pulp was adjusted to about 5.0 with a 30% aluminum sulfate solution, and then rosin glue was added. After stirring for 1 minute, talcum powder was added, and after stirring for 1 minute, a retention agent was added. After 1 minute, the prepared pulp was removed, and sheets were made with a 73-62 semi-automatic paper sheet former, and after being pressed with a 73-50 standard paper sheet press, the paper sample was dried with a glazing machine, and the 1-minute Cobb value of the paper sample was tested. The test results are shown in Table 1.
[0045] Table 1 Test results of water absorption performance of paper after sizing with different sizing agents
[0046]
[0047]
[0048] Judging from the water absorption value of hand-sheet paper samples, the water resistance of the sizing agent prepared by replacing part of the cationic rosin with furfural urea resin and using all cationic rosin was not significantly reduced but enhanced.
[0049] It should be understood by those skilled in the art that the above embodiments are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functions and principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be modified or altered in any way without departing from the principles.
Claims
1. A cationic rosin / furfural urea resin composite sizing agent, characterized in that: The invention is composed of cationic rosin, furfural urea resin and an appropriate amount of emulsifier, and the preparation method thereof comprises the following steps: S1, 120 g urea and 1000 g maltose were added to the reactor, stirring was started, the temperature was raised to 90°C, metal ion catalyst magnesium acetate was added, the reaction time was 8 h, and the temperature was cooled to room temperature to obtain furfural urea resin; S2, adding 95g of rosin into a reactor, heating to 180°C, and then adding 7.6g of maleic anhydride and fumaric acid to modify the rosin to obtain cationic rosin, wherein the maleic anhydride and fumaric acid are compounded in a mass ratio of 1:1; S3, cooling to 120 ℃, adding the furfural urea resin in an amount of 19g, after mixing, adding 28.5g of composite cationic emulsifier under high-speed stirring, the temperature is 60 ℃, after stirring, adding hot water to invert the phase, controlling the speed to 1800rpm / min during the phase inversion, adjusting the solid content to 40%, cooling to room temperature, and obtaining a cationic rosin / furfural urea resin composite sizing agent; the composite cationic emulsifier adopts a composite emulsifier of cationic quaternary ammonium salt surfactant and polyamide polyamine epichlorohydrin, wherein the cationic quaternary ammonium salt surfactant accounts for 20% of the total weight of the composite emulsifier.