Composite conductive particles and preparation method and application
By using composite conductive particles composed of nanobarium titanate and conductive graphite powder in waste lithium battery recycling, the problems of safety hazards and environmental pollution in lithium battery recycling are solved, and safe and efficient discharge treatment is achieved, suitable for large-scale Production.
Patent Information
- Application Number
- CN202310886287.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-07-18
AI Technical Summary
There are safety hazards and environmental pollution problems in the recycling of existing waste lithium batteries. They are prone to fire or explosion when physically crushed, and the discharge efficiency of salt water is low and secondary pollution is generated, making it difficult to adapt to large-scale production.
Compound conductive particles are used to mix nanobarium titanate compounds with nano-inorganic powder, and conductive graphite powder is added to form temperature-controlled composite conductive particles with core-shell structures. They are used for discharge treatment of waste lithium batteries to achieve initial room temperature discharge, Medium-term heat dissipation and rapid and safe discharge in the later stage to avoid heat loss.
It realizes safe and controllable discharge of waste lithium batteries, reduces the risks of fire and explosion, avoids dust pollution, improves discharge efficiency, and is suitable for large-scale industrial production.
Smart Images

Figure CN116705379B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste lithium battery recycling, and specifically relates to composite conductive particles for recycling and discharging waste lithium batteries, and a preparation method and application thereof. Background Art
[0002] The actual retirement time of power lithium batteries is about 5 to 8 years. After some batteries are retired, they are reused for 2 years before entering the scrapping stage. As the amount of scrapped lithium batteries continues to increase, the comprehensive recycling of waste lithium batteries is urgent. According to relevant agencies, it is expected that the total amount of retired power batteries in my country will reach 137.4GWh in 2025, and the output value of cascade utilization and recycling is expected to exceed 100 billion yuan. It is predicted that by 2025, the recycling capacity of waste batteries in China will reach 960,000 tons, and the amount of lithium, cobalt, nickel, manganese and other resources that can be recycled through power battery recycling will account for approximately 27.7%, 55.5%, 28.7% and 47.9% of the corresponding demand, respectively. Therefore, recycling waste lithium batteries has great economic value. However, waste lithium batteries still have a lot of energy, and there are safety hazards of combustion and explosion during storage, transportation and disassembly and recycling. Therefore, how to safely and effectively recycle waste lithium batteries is an urgent problem to be solved. The first step in recycling waste lithium batteries is to discharge them efficiently and safely to reduce safety hazards.
[0003] At present, there are great safety hazards in the physical crushing of waste lithium-ion battery recycling. The residual electricity of waste lithium batteries can easily cause instantaneous conductive short circuits in the positive and negative electrode materials when crushed, releasing a large amount of heat, igniting the low-flash-point organic electrolytes in the battery, inducing further exothermic reactions, leading to thermal runaway, and ultimately causing fire or explosion. Even if physical crushing is carried out under the protection of an inert atmosphere or low-temperature cold air, it is difficult to avoid the subsequent risk of spontaneous combustion of negative electrode graphite dust due to oxygen storage, which also poses a safety hazard. Therefore, it is an industry consensus that waste lithium-ion batteries must be discharged before crushing to release residual electricity.
[0004] The most commonly used discharge method for recycling waste lithium batteries in the prior art is to use salt water discharge. Salt water discharge has the advantages of simple process and low discharge cost, but salt water discharge does have serious environmental pollution problems. Salt water discharge is to soak the battery in a certain concentration of sodium chloride or sodium sulfate solution, and use stirring and other methods to make the battery undergo ion conduction and electrolysis reaction, and finally complete the discharge process. Salt water discharge will produce a large amount of hydrogen, chlorine, oxygen, etc., causing secondary pollution to the surrounding environment; after multiple discharges of salt water, it will cause serious electrochemical corrosion to the steel shell, aluminum shell, positive aluminum foil, negative copper foil, pole piece active material, pole ear, etc. of the waste lithium battery, and it is easy to introduce a large amount of impurity anions and cations, and often contains a large amount of brown flocculent precipitates, which will cause secondary pollution, which will have a great impact on the subsequent removal and separation of valuable metals. Purification, the extraction process of valuable metals is more complicated, and the cost of impurity removal is greatly increased. In addition, the efficiency of salt water discharge is low, the discharge cycle is 3 to 5 days, the production efficiency is low, and it is not suitable for the control of large-scale modern enterprise production processes.
[0005] At present, there is also a physical discharge method using an external load, where a number of used batteries are connected in parallel through a battery fixture, and the positive and negative electrodes of the batteries are connected and conducted to the external circuit respectively. This external discharge method requires the used batteries to be arranged regularly, and each single battery is equipped with a connection line. Since the residual energy of each single battery is different, the discharge progress needs to be monitored separately, which not only increases the cost of the discharge process, but also has the potential safety hazard of thermal polymerization and flammability during the discharge process, which does not meet the production requirements of large-scale solid waste treatment of used lithium-ion batteries.
[0006] Therefore, it is necessary to solve the above problems. Summary of the invention
[0007] The purpose of the present invention is to overcome the above-mentioned deficiencies in the prior art, and firstly provides a composite conductive particle.
[0008] The composite conductive particles provided by the invention comprise the following raw materials in percentage by mass: 10-20% of nanometer barium titanate compound powder, 0.1-1.0% of nanometer inorganic powder, 3-10% of adhesive, and 70-85% of conductive graphite powder.
[0009] The present invention also provides a method for preparing the composite conductive particles, comprising the following steps:
[0010] S1. Evenly mixing nano-barium titanate compound powder and nano-inorganic powder, and performing vacuum heating treatment to obtain hybrid nano-composite dielectric ceramic powder;
[0011] S2: mixing an adhesive and a solvent to dissolve into a liquid adhesive, then adding the nano-composite dielectric ceramic powder, and fully dispersing and mixing the nano-inorganic powder in the adhesive by high-speed shear dispersion, ultrasonic dispersion and grinding to form a nano-composite dielectric ceramic slurry;
[0012] S3: mixing conductive graphite powder into the nanocomposite dielectric ceramic slurry, uniformly dispersing the powder and then extruding and granulating the powder;
[0013] S4 is made into composite conductive particles after heating treatment.
[0014] The present invention also provides the use of the composite conductive particles prepared by the composite conductive particle preparation method described above in the recycling of waste lithium batteries.
[0015] The invention uniformly mixes barium titanate compound powder and nano inorganic powder, heats to obtain mixed nano composite dielectric ceramic powder, disperses and grinds to form nano composite dielectric ceramic slurry, and then adds conductive graphite powder to the nano composite dielectric ceramic slurry in batches, so that the conductive graphite powder and the nano composite dielectric ceramic slurry are fully contacted, dissociated, adsorbed, dispersed and homogeneously mixed, and under the adhesion of an adhesive, the nano composite dielectric ceramic powder is completely wrapped by the conductive graphite powder to form composite conductive particles with a core-shell structure. The invention utilizes the temperature-sensitive jump characteristic of the dielectric constant of barium titanate materials, combines nano inorganic powder, and makes the dielectric powder of nano barium titanate compounds and the nano inorganic powder melt into the tetragonal crystal structure of barium titanate in the solid phase sintering process, so that the metal elements of the nano inorganic powder are diffused, replaced or embedded in the barium titanate compound structure, so that the barium titanate compound structure is distorted, and the Curie temperature (Tc) of the original barium titanate compound is changed, so that the prepared composite conductive particles have both the temperature-sensitive resistance jump characteristic of the dielectric material and the high conductivity characteristic, and the resistivity will show an increasing change with the temperature change, and the resistivity is between 5 and 15Ω·cm at room temperature; the Curie temperature Tc is between 40 and 50°C.
[0016] The composite conductive particles of the present invention are characterized in that the inner core is a low-resistance composite dielectric ceramic particle, and the outer shell is a highly conductive graphite. At room temperature, the conductive graphite completely wraps the ceramic particles, mainly exerting the conductive performance. In an environment that breaks through the Curie temperature, the inner core composite dielectric material absorbs heat to achieve chemical cross-linking. When applied to the discharge treatment process of waste lithium-ion batteries, it can achieve room temperature discharge in the early stage, high-temperature heat dissipation in the middle stage, and rapid and safe discharge in the late stage. The heat generated in the discharge process is effectively evacuated, avoiding local thermal runaway and fire, explosion and other safety hazards. In addition, the composite conductive particles are not easy to shed powder when used, and will not generate dust pollution, and can be reused.
[0017] The invention has simple process and low cost, and the discharge process of waste lithium batteries is safe and controllable, which is conducive to industrial large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a block diagram of an embodiment of the method for preparing composite conductive particles of the present invention. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0020] The invention firstly provides a temperature-controlled composite conductive particle, which comprises the following raw materials in percentage by mass: 10-20% of nanometer barium titanate compound powder, 0.1-1.0% of nanometer inorganic powder, 3-10% of adhesive, and 70-85% of conductive graphite powder.
[0021] The barium titanate compound of the present invention can be selected from any one of BaTi3O7, BaTiSiO5, BaAlSi2O6 or BaCaTi3O3. These raw materials are strong dielectric compound materials with high dielectric constant, low dielectric loss and temperature-sensitive jump characteristics, and are not easy to oxidize, corrosion-resistant and have stable performance; the nano inorganic powder can be selected from conductive metal materials, including any one of silver, tin, nickel, zirconium, antimony oxide or zirconium oxide; the conductive graphite has high conductivity; the adhesive can be selected from any one of EA epoxy glue, PVC polyvinyl alcohol or CMC sodium hydroxymethyl cellulose glue with better adhesion effect. The above adhesive has strong adhesion and has high dielectric properties, excellent mechanical properties and chemical stability after curing.
[0022] The present invention mixes nano-barium titanate dielectric powder with nano-inorganic powder, so that during the solid-phase sintering process, the conductive metal particles can be embedded in the lattice of the barium titanate compound, making it easier to become a semiconductor, and is used to reduce the room temperature resistivity. By adding an adhesive, a nano-composite dielectric ceramic slurry can be formed, and then coated with conductive graphite powder, the nano-composite dielectric ceramic particles are embedded in the conductive graphite powder through the adhesive effect, forming composite conductive particles with core-shell structure characteristics. The core of this composite conductive particle is a low-resistance composite dielectric ceramic particle, and the shell is a highly conductive graphite. At room temperature, the conductive graphite completely wraps the ceramic particle. The dielectric constant temperature change characteristics of the mixture of nano-barium titanate compound dielectric powder and nano-inorganic powder and the high conductivity characteristics of the conductive graphite are used to synergistically exert the characteristics of each material, so that the composite conductive particle has both the temperature-sensitive resistance jump characteristics of the dielectric material and the high conductivity characteristics, which can ensure the completeness of the discharge. At the same time, the resistivity can change in a step-by-step manner with the change of temperature. At room temperature, the resistivity of the composite conductive particle is between 5 and 15Ω·cm, and the Curie temperature Tc is between 40 and 50℃; when the environment is higher than the Curie temperature, the resistivity increases by 102 ~10 3 The order of magnitude increases, so that the conduction discharge process slows down or stops, so as to reduce the potential risks caused by rapid temperature rise during continuous discharge. In this way, the composite conductive particles of the present invention can achieve initial room temperature discharge, mid-term heat dissipation and late room temperature rapid discharge during the discharge treatment process when used in the recycling of waste lithium-ion batteries, forming automatic intermittent discharge. The whole process is very safe, controllable, and the discharge is complete.
[0023] See also Figure 1 The present invention also provides a method for preparing the composite conductive particles, comprising the following steps:
[0024] S1 Firstly, nano-barium titanate compound powder and nano-inorganic powder are uniformly mixed, and then vacuum-heated to obtain hybrid nano-composite dielectric ceramic powder.
[0025] In this step, the barium titanate compound is selected from BaTi3O7, BaTiSiO5, BaAlSi2O6 or BaCaTi3O3, and the nano inorganic powder is silver, tin, nickel, zirconium, antimony oxide or zirconium oxide. The mass ratio of the nano barium titanate compound powder is 95% to 99%, and the powder particle size is less than 200nm; the mass percentage of the nano inorganic powder is 1% to 5%, and the average powder particle size is less than 60nm.
[0026] In this step, the barium titanate powder and the nano inorganic powder are mechanically mixed, and a dispersing device combining shear dispersion and convection dispersion is selected, and high-speed stirring (800-1100rpm) is used to disperse evenly, so that the raw materials are fully contacted, scattered, depolymerized and orderly mixed, and then vacuum sintering and heating treatment are carried out. The heating temperature and insulation time vary according to the type of inorganic powder. The heating temperature is 100-1500°C and the insulation time is 10-60min to obtain a hybrid nano composite dielectric ceramic powder.
[0027] In this step, during the sintering and heating treatment process in a vacuum environment, the metastable nano-inorganic powder is attached to the surface of the nano-barium titanate compound. When the heating temperature is close to the melting point of the nano-inorganic powder material, it begins to change from solid to liquid. Liquid metal ions or atoms diffuse, replace or embed into the two-phase interface, the crystal boundary of the nano-barium titanate compound and the interior of its lattice through molecular thermal motion. Even smaller nano-metal ions can partially replace titanium ions or calcium ions in the parent square lattice, causing the crystal structure of the barium titanate compound to be distorted, reducing the original nano-barium titanate lattice parameter ratio (c / a). Metal ion doping makes the barium titanate compound crystal semiconductor, the resistivity is reduced, and the Curie peak of the composite dielectric particles moves to a low temperature, changing the Curie temperature (Tc) of the original barium titanate compound, reducing the Curie temperature from 120°C to between 40 and 50°C, thereby obtaining low-resistivity composite dielectric ceramic powder particles.
[0028] S2: Mix the adhesive and the solvent in a certain proportion and dissolve them into a liquid adhesive, then add the nano-composite dielectric ceramic powder, and fully disperse and mix the nano-inorganic powder in the adhesive by high-speed shear dispersion, ultrasonic dispersion and grinding to form a nano-composite dielectric ceramic slurry. The mass ratio of the nano-composite dielectric ceramic powder, the adhesive and the solvent is 10:2 to 7:2 to 10. The solvent is selected from any one of water, ethanol, methanol or acetone.
[0029] In this step, an adhesive and a solvent are added to the nano-composite dielectric ceramic powder, and then high-speed shear stirring is adopted. The stirring speed during high-speed shear dispersion is 800-1100 rpm and the time is 3-5 hours. Ultrasonic dispersion is then performed for 1-3 hours, and then grinding is performed for 3-5 hours. In this way, the nano-metal particles can be further embedded in the clustered barium titanate compound particles, and the composite dielectric material and the polymer adhesive can be fully contacted, entangled and bonded to form a nano-composite dielectric ceramic slurry that is evenly dispersed, stable, homogeneous and viscous.
[0030] S3: mixing conductive graphite powder into the nanocomposite dielectric ceramic slurry, uniformly dispersing the powder and then extruding and granulating the powder into a shape.
[0031] In this step, the mass percentage of the nanocomposite dielectric ceramic slurry added is 20% to 40%; the mass percentage of the conductive graphite powder added is 60 to 80%, and the average particle size of the conductive graphite powder is 6.5 to 18 μm. To ensure uniform dispersion, the conductive graphite powder can be added three times, and the amount added each time is 1 / 3 of the total amount of the conductive graphite powder.
[0032] In this step, a certain proportion of conductive graphite powder is added to the nano-composite dielectric ceramic slurry, and the conductive graphite powder is added to the quantitative nano-composite dielectric ceramic slurry in batches by shear mixing and diffusion mixing through high shear dispersion equipment, so that the conductive graphite powder and the nano-composite dielectric ceramic slurry are fully contacted and chemically adsorbed, so that the nano-composite dielectric ceramic powder particles are coated layer by layer in the conductive graphite powder through adhesion to form stepped core-shell structure particles, and then made into spherical, elliptical, cylindrical or cubic particles through an extrusion machine.
[0033] S4 is heated to produce denser solid composite conductive particles.
[0034] In this step, the particles after extrusion granulation are further heated and dried at a temperature of 80 to 100°C for 20 to 60 minutes. The solvent can be removed and further heat-condensed to obtain a more compact, stepped, and temperature-controlled composite conductive particle with core-shell structure. The prepared composite conductive particles have a Curie temperature of 40 to 50°C and a resistivity of 5 to 15Ω·cm at room temperature. When the ambient temperature is above 45°C, the resistivity is increased to 10 2 ~10 3 Ω·cm or more.
[0035] The preparation method has simple process, low cost and is conducive to industrial large-scale production.
[0036] The present invention also provides the use of the composite conductive particles prepared by the composite conductive particle preparation method in the recycling of waste lithium batteries.
[0037] The composite conductive particles of the present invention can be mixed with waste lithium batteries in an orderly manner to achieve physical discharge. Specifically, a layered sandwich physical contact method can be adopted, where a layer of the composite conductive particles of the present invention is spread on each single layer of waste lithium batteries, and then another layer of waste lithium batteries is placed, and the waste lithium battery monomers in the same row are arranged side by side and closely and neatly, and the spacing between each row of batteries is greater than the diameter of the composite conductive particles. After each layer of waste lithium batteries is laid, composite conductive particles are added to the spacing between the waste lithium battery rows to fill the gaps between the waste lithium batteries, so that the positive and negative electrodes of the waste lithium battery monomers are in contact with sufficient composite conductive particles, and then another layer of composite conductive particles is spread, ..., and so on and so forth, and the last layer is composite conductive particles. At the same time, a certain external pressure can be applied to make the composite conductive particles of the present invention fully and closely contact the positive and negative electrodes of the waste lithium battery monomers, so that the positive and negative electrodes of the waste lithium batteries can be connected with the help of the composite conductive particles, forming a conductive path, thereby achieving temperature-controlled physical discharge.
[0038] The preparation method and application of the composite conductive particles are further described in detail below in conjunction with specific embodiments. Example 1
[0039] 1. Preparation of composite conductive particles:
[0040] S1 puts 99 grams of nano BaTi3O7 powder (particle size less than 200nm) and 1 gram of nano silver (particle size <60nm) powder into a mixer, and mixes the two powders fully under the action of high-speed stirring shear (stirring speed 1000rpm, mixing time 2 hours) shearing and repeated displacement diffusion stirring. Then, the mixed powder is put into a tubular electric furnace for vacuum heating treatment at 100°C for 20 minutes. After naturally cooling to room temperature, a hybrid nano composite dielectric ceramic powder is obtained.
[0041] S2: 80 g of EA epoxy glue and 100 g of acetone solvent are mixed and dissolved into a liquid glue solution, and then 100 g of nano-composite dielectric ceramic powder prepared in step S1 is added, firstly stirred at 800 rpm for 30 min, then ultrasonically dispersed for 60 min, and then stirred and dispersed at 1000 rpm for 2.5 h, and finally ground in a ball mill for 3 h, so that the flexible nano-silver particles are further embedded in the clustered nano-BaTi3O7 particles, and the composite dielectric material and the polymer adhesive are fully contacted, entangled and bonded to form a uniformly dispersed, stable, homogeneous and viscous nano-composite dielectric ceramic slurry.
[0042] S3 adds 720 grams of conductive graphite powder (average particle size 10 μm) into 230 grams of nano-composite dielectric ceramic slurry in three equal batches, and utilizes the strong stirring action of high-speed shear dispersion equipment to fully contact, dissociate, adsorb, disperse and homogenize the conductive graphite powder and nano-composite dielectric ceramic slurry. With the help of the adhesion of the adhesive, the nano-composite dielectric ceramic powder is coated layer by layer (three times) by the conductive graphite powder. According to the component distribution characteristics, stepped core-shell structured composite conductive particles are formed, and then further kneaded, homogenized and mixed through the rotating twin-screw extrusion action of the extrusion granulator. After pressurized transportation, nearly spherical composite conductive particles are extruded from the template holes.
[0043] S4 The spherical composite conductive particles obtained in step S3 are placed in a vacuum drying oven, heated and dried at 80°C for 40 minutes to remove the solvent and further heat condense to obtain denser, stepped and temperature-controlled composite conductive particles with core-shell structure characteristics. The room temperature resistivity of the composite conductive particles is about 5Ω·cm, and the Curie temperature Tc is 47°C.
[0044] 2. Application of composite conductive particles in lithium battery recycling
[0045] The 1000 g of the prepared composite conductive particles were orderly mixed with 20 waste lithium battery monomers. A sandwich-type layered mixing method was used. First, 300 g of the composite conductive particles were added to the bottom of the material frame to form a conductive medium layer. Then two rows of waste lithium batteries were placed, with 5 batteries in each row, a total of 10 lithium batteries, with an interval of 1 to 3 cm. Then 400 g of the composite conductive particles were spread again, and then a layer of lithium battery monomers was added, with a total of 10 batteries in two rows, and the spacing was still 1 to 3 cm. Finally, the remaining 300 g of the composite conductive particles were added, and then a packaging plastic plate was added on the material frame. A certain pressure was applied to the upper end to make the composite conductive particles fully and closely contact with the waste lithium-ion batteries, and then placed still for safe discharge.
[0046] The room temperature resistivity of the composite conductive particles in this embodiment is 5Ω·cm, and the discharge time is less than 1 hour. Example 2
[0047] 1. Preparation of composite conductive particles:
[0048] S1 puts 147 grams of nano BaTiSiO5 powder (particle size less than 200nm) and 3 grams of nano tin (particle size <60nm) powder in a mixer, and fully mixes the two powders under the action of strong gas convection and high-speed stirring (stirring speed 1300rpm, mixing time 1.5 hours). Then, the mixed powder is put into a tubular electric furnace and vacuum heated at 240℃ for 10min. Then, it is naturally cooled to room temperature to obtain a hybrid nano-composite dielectric ceramic powder.
[0049] S2: 45 grams of polyvinyl alcohol and 100 grams of ethanol are mixed and dissolved into a liquid glue, and then 150 grams of nano-composite dielectric ceramic powder prepared in step S1 is added. First, stirring is performed at 900 rpm for 60 minutes, and then ultrasonic dispersion treatment is performed for 90 minutes, and then stirring and dispersing is performed at 1000 rpm for 1.5 hours. Finally, it is placed in a ball mill for grinding for 4 hours to further embed the flexible nano-tin particles into the clustered BaTiSiO5 particles, and to allow the composite dielectric material and the polymer adhesive to be fully contacted, entangled and bonded to form a uniformly dispersed, stable, homogeneous and viscous nano-composite dielectric ceramic slurry.
[0050] S3 adds 705 grams of conductive graphite powder (average particle size 15μm) into 295 grams of composite dielectric ceramic slurry in three equal batches, and utilizes the strong stirring action of high-speed shear dispersion equipment to fully contact, dissociate, adsorb, disperse and homogenize the conductive graphite powder and nano-composite dielectric ceramic slurry. With the help of the adhesion of the adhesive, the nano-composite dielectric ceramic powder is coated layer by layer (three times) by the conductive graphite powder. According to the component distribution characteristics, stepped core-shell structured composite conductive particles are formed, and then further kneaded, homogenized and mixed through the rotating twin-screw extrusion action of the extrusion granulator. After pressurized transportation, nearly spherical composite conductive particles are extruded from the template holes.
[0051] S4 The spherical composite conductive particles obtained in step S3 are placed in a vacuum drying oven, heated and dried at 100°C for 10 minutes to remove the solvent and further thermally polymerize to obtain denser, stepped and temperature-controlled composite conductive particles with core-shell structure characteristics. The room temperature resistivity of the composite conductive particles is about 8Ω·cm, and the Curie temperature Tc is 42°C.
[0052] 2. Application of composite conductive particles in lithium battery recycling
[0053] The 1000 g of the prepared composite conductive particles were orderly mixed with 30 waste lithium battery monomers. A sandwich-type layered mixing method was used. First, 300 g of the composite conductive particles were added to the bottom of the material frame to form a conductive medium layer. Then 3 rows of waste lithium batteries were placed, with 5 batteries in each row, a total of 15 lithium batteries, with an interval of 1 to 3 cm. Then 400 g of the composite conductive particles were spread again, and then a layer of lithium battery monomers was added, with a total of 15 batteries in 3 rows, and the spacing was still 1 to 3 cm. Finally, the remaining 300 g of the composite conductive particles were added, and then a packaging plastic plate was added on the material frame. A certain pressure was applied to the upper end to make the composite conductive particles fully and closely contact with the waste lithium-ion batteries, and then placed still for safe discharge.
[0054] The room temperature resistivity of the composite conductive particles in this embodiment is 8Ω·cm, and the discharge time is less than 1.5 hours. Example 3
[0055] 1. Preparation of composite conductive particles:
[0056] S1 puts 116.4 grams of nano BaAlSi2O6 powder (particle size less than 200nm) and 3.6 grams of nano nickel (particle size <60nm) powder into a mixer, and fully mixes the two powders under the action of strong gas convection and high-speed shear stirring (stirring speed 1300rpm, mixing time 1 hour). Then, the mixed powder is put into a tubular electric furnace for vacuum heating treatment at 800℃ for 60min, and then naturally cooled to room temperature to obtain a hybrid nano composite dielectric ceramic powder.
[0057] S2: 30 g of PVC glue and 50 g of acetone solvent are mixed and dissolved into a liquid glue solution, and then 120 g of the nano-composite dielectric ceramic powder prepared in step S1 is added, and first stirred at 800 rpm for 30 min, and then ultrasonic dispersion treatment is performed for 60 min, followed by stirring and dispersion at 1000 rpm for 2.5 h, and finally ground in a ball mill for 3 h, so that the flexible nano-nickel particles are further embedded in the clustered nano-BaAlSi2O6 particles, and the composite dielectric material and the polymer adhesive are fully contacted, entangled and bonded to form a uniformly dispersed, stable, homogeneous and viscous nano-composite dielectric ceramic slurry.
[0058] S3 Add 800 grams of conductive graphite powder (average particle size 18μm) into 200 grams of composite dielectric ceramic slurry in three equal batches. Use the strong stirring action of high-speed shear dispersion equipment to make the conductive graphite powder and nano-composite dielectric ceramic slurry fully contact, dissociate, adsorb, disperse and homogenize. With the help of the adhesion of the adhesive, the nano-composite dielectric ceramic powder is coated layer by layer by the conductive graphite powder (three times of coating). According to the distribution characteristics of the components, stepped core-shell composite conductive particles are formed. Then, they are further kneaded, homogenized and mixed through the rotating twin-screw extrusion action of the extrusion granulator. After pressurized transportation, nearly spherical particles are extruded from the template holes.
[0059] S4 The spherical composite conductive particles obtained in step S3 are placed in a vacuum drying oven, heated and dried at 80°C for 20 minutes to remove the solvent and further heat condense to obtain denser, stepped and temperature-controlled composite conductive particles with core-shell structure characteristics. The room temperature resistivity of the composite conductive particles is about 12Ω·cm, and the Curie temperature Tc is 48°C.
[0060] 2. Application of composite conductive particles in lithium battery recycling
[0061] The 1000 g of the prepared composite conductive particles were orderly mixed with 24 waste lithium battery monomers. A sandwich-type layered mixing method was used. First, 300 g of the composite conductive particles were added to the bottom of the material frame to form a conductive medium layer. Then two rows of waste lithium batteries were placed, with 6 batteries in each row, a total of 12 lithium batteries, with an interval of 1 to 3 cm. Then 400 g of the composite conductive particles were spread again, and then a layer of lithium battery monomers was added, with a total of 12 batteries in two rows, and the interval was still 1 to 3 cm. Finally, the remaining 300 g of the composite conductive particles were added, and then a packaging plastic plate was added to the material frame, and a certain pressure was applied to the upper end to make the composite conductive particles fully and closely contact with the waste lithium-ion batteries, and then placed still for safe discharge.
[0062] The room temperature resistivity of the composite conductive particles in this embodiment is 12Ω·cm, and the discharge time is less than 2 hours. Example 4
[0063] 1. Preparation of composite conductive particles:
[0064] S1 puts 190 grams of nano-BaCaTi3O3 powder (particle size less than 200nm) and 8 grams of nano-zirconium powder (particle size <50nm) into a mixer, and mixes the two powders fully under the stirring action of strong gas convection and high-speed shear (stirring speed 1200rpm, mixing time 1.5 hours). Then, the mixed powder is put into a tubular electric furnace for vacuum heating treatment at 1500℃ for 60min, and then naturally cooled to room temperature to obtain a hybrid nano-composite dielectric ceramic powder.
[0065] S2: 70 g of EA epoxy glue and 130 g of ethanol solvent are mixed and dissolved into a liquid glue solution, and then 100 g of the nano-composite dielectric ceramic powder prepared in step S1 is added, and first stirred at 800 rpm for 30 min, and then ultrasonic dispersion treatment is performed for 60 min, and then stirring and dispersing is performed at 1000 rpm for 2.5 h, and finally grinding is performed in a ball mill for 5 h, so that the flexible nano-zirconium particles are further embedded in the clustered BaCaTi3O3 particles, and the composite dielectric material and the polymer adhesive are fully contacted, entangled and bonded to form a uniformly dispersed, stable, homogeneous and viscous nano-composite dielectric ceramic slurry.
[0066] S3 added 682 grams of conductive graphite powder (average particle size 18μm) into 230 grams of composite dielectric ceramic slurry in three equal batches, and used the strong stirring action of high-speed shear dispersion equipment to make the conductive graphite powder and nano-composite dielectric ceramic slurry fully contact, dissociate, adsorb, disperse and homogeneously mix. With the help of the adhesion of the adhesive, the nano-composite dielectric ceramic powder was coated layer by layer (three times) by the conductive graphite powder. According to the component distribution characteristics, stepped core-shell structured composite conductive particles were formed, and then further kneaded, homogenized and mixed through the rotating twin-screw extrusion action of the extrusion granulator. After pressurized transportation, nearly spherical composite conductive particles were extruded from the template holes.
[0067] S4 The spherical composite conductive particles obtained in step S3 are placed in a vacuum drying oven, heated and dried at 100°C for 120 minutes to remove the solvent and further thermally polymerize to obtain denser, stepped and temperature-controlled composite conductive particles with core-shell structure characteristics. The room temperature resistivity of the composite conductive particles is about 15Ω·cm, and the Curie temperature Tc is 46°C.
[0068] 2. Application of composite conductive particles in lithium battery recycling
[0069] The 1000 g of the prepared composite conductive particles were orderly mixed with 20 waste lithium battery monomers. A sandwich-type layered mixing method was used. First, 300 g of the composite conductive particles were added to the bottom of the material frame to form a conductive medium layer. Then two rows of waste lithium batteries were placed, with 5 batteries in each row, a total of 10 lithium batteries, with an interval of 1 to 3 cm. Then 400 g of the composite conductive particles were spread again, and then a layer of lithium battery monomers was added, with a total of 10 batteries in two rows, and the interval was still 1 to 3 cm. Finally, the remaining 300 g of the composite conductive particles were added, and then a packaging plastic plate was added to the material frame, and a certain pressure was applied to the upper end to make the composite conductive particles fully and closely contact with the waste lithium-ion batteries. The frame was placed still for safe discharge.
[0070] The room temperature resistivity of the composite conductive particles in this embodiment is 15Ω·cm, and the discharge time is less than 2.5 hours. Example 5
[0071] 1. Preparation of composite conductive particles:
[0072] S1 98 grams of nano BaTi3O7 powder (particle size less than 200nm) and 2 grams of nano antimony oxide (particle size <60nm) powder are placed in a mixer, and the two powders are fully mixed under the action of strong gas convection and high-speed shear stirring (stirring speed 1100rpm, mixing time 2 hours). The mixed powder is then placed in a tubular electric furnace and vacuum heated at 460°C for 30 minutes. The mixture is then naturally cooled to room temperature to obtain a hybrid nano-composite dielectric ceramic powder.
[0073] S2: 60 grams of PVC and 100 grams of acetone solvent are mixed and dissolved into a liquid glue, and then 100 grams of nano-composite dielectric ceramic powder prepared in step S1 is added, firstly stirred at 800 rpm for 30 minutes, and then ultrasonic dispersion treatment is carried out for 60 minutes, followed by stirring and dispersion at 1000 rpm for 2.5 hours, and finally ground in a ball mill for 5 hours, so that the flexible nano-antimony oxide particles are further embedded in the clustered BaTi3O7 particles, and the composite dielectric material and the polymer adhesive are fully contacted, entangled and bonded to form a uniformly dispersed, stable, homogeneous and viscous nano-composite dielectric ceramic slurry.
[0074] S3 adds 740 grams of conductive graphite powder (average particle size 8 μm) into 260 grams of composite dielectric ceramic slurry in three equal batches, and utilizes the strong stirring action of high-speed shear dispersion equipment to fully contact, dissociate, adsorb, disperse and homogenize the conductive graphite powder and nano-composite dielectric ceramic slurry. With the help of the adhesion of the adhesive, the nano-composite dielectric ceramic powder is coated layer by layer (three times) by the conductive graphite powder, and according to the component distribution characteristics, a stepped core-shell structure composite conductive particle is formed, which is then further kneaded, homogenized and mixed through the rotating twin-screw extrusion action of the extrusion granulator, and pressed and conveyed to extrude nearly spherical particles from the template hole.
[0075] S4 The spherical composite conductive particles obtained in step S3 are placed in a vacuum drying oven, heated and dried at 80°C for 30 minutes to remove the solvent and further heat condense to obtain denser, stepped and temperature-controlled composite conductive particles with core-shell structure characteristics. The room temperature resistivity of the composite conductive particles is about 13Ω·cm, and the Curie temperature Tc is 43°C.
[0076] 2. Application of composite conductive particles in lithium battery recycling
[0077] The 1000 g of the prepared composite conductive particles were orderly mixed with 20 waste lithium battery monomers. A sandwich-type layered mixing method was used. First, 300 g of the composite conductive particles were added to the bottom of the material frame to form a conductive medium layer. Then two rows of waste lithium batteries were placed, with 5 batteries in each row, a total of 10 lithium batteries, with an interval of 1 to 3 cm. Then 400 g of the composite conductive particles were spread again, and then a layer of lithium battery monomers was added, with a total of 10 batteries in two rows, and the interval was still 1 to 3 cm. Finally, the remaining 300 g of the composite conductive particles were added, and then a packaging plastic plate was added to the material frame, and a certain pressure was applied to the upper end to make the composite conductive particles fully and closely contact with the waste lithium-ion batteries, and then placed still for safe discharge.
[0078] The room temperature resistivity of the composite conductive particles in this embodiment is 13Ω·cm, and the discharge time is less than 2 hours.
[0079] The above-mentioned embodiments of the present invention are only part of the preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made by those skilled in the art without departing from the essence of the present invention are within the protection scope of the present invention.
Claims
1. A composite conductive particle comprising the following raw materials in the following mass percentages: 10-20% nano-barium titanate compound powder, 0.1-1.0% nano-inorganic powder, 3-10% adhesive, 70-85% conductive graphite powder; wherein the nano-inorganic powder is any one of silver, tin, nickel, zirconium, antimony oxide or zirconium oxide; The preparation method comprises the following steps: S1. Evenly mixing nano-barium titanate compound powder and nano-inorganic powder, and performing vacuum heating treatment to obtain hybrid nano-composite dielectric ceramic powder; S2: mixing an adhesive and a solvent to dissolve them into a liquid adhesive, then adding the nanocomposite dielectric ceramic powder, and fully dispersing and mixing the nano inorganic powder in the adhesive by high-speed shear dispersion, ultrasonic dispersion, and grinding to form a nanocomposite dielectric ceramic slurry; S3: mixing conductive graphite powder into the nanocomposite dielectric ceramic slurry in batches, uniformly dispersing the powder and then extruding and granulating the powder; S4 is made into composite conductive particles after heat treatment.
2. The composite conductive particle according to claim 1, wherein The barium titanate compound powder is any one of BaTi3O7, BaTiSiO5, BaAlSi2O6 or BaCaTi3O3. The nano inorganic powder is any one of silver, tin, nickel, zirconium, antimony oxide or zirconium oxide.
3. The composite conductive particle according to claim 1 or 2, characterized in that: The adhesive is any one of EA epoxy glue, PVC, polyvinyl alcohol or CMC sodium hydroxymethyl cellulose glue.
4. The composite conductive particle according to claim 1, wherein In step S1 of the preparation method, the mass ratio of the nano-barium titanate compound powder is 95% to 99%, and the powder particle size is less than 200 nm; the mass ratio of the nano-inorganic powder is 1% to 5%, and the average particle size is less than 60 nm.
5. The composite conductive particle according to claim 1 or 4, characterized in that: In step S1 of the preparation method, the barium titanate compound powder and the nano inorganic powder are subjected to convection and shear stirring to fully contact, scatter, deagglomerate and orderly mix the raw materials, and then vacuum sintering and heating treatment are performed at a heating temperature of 100 to 1500° C. and a holding time of 10 to 60 minutes.
6. The composite conductive particle according to claim 1, wherein In step S2 of the preparation method, the mass ratio of the nanocomposite dielectric ceramic powder, the adhesive, and the solvent is 10:2 to 7:2 to 10.
7. The composite conductive particle according to claim 1 or 6, characterized in that: In step S2 of the preparation method, the stirring speed during high-speed shear dispersion is 800-1100 rpm, and the time is 3-5 hours; the ultrasonic dispersion time is 1-3 hours; and the grinding dispersion time is 3-5 hours.
8. The composite conductive particle according to claim 1, wherein In step S3 of the preparation method, the conductive graphite powder has an average particle size of 6.5 to 18 μm, and the conductive graphite powder is added in three times, with the amount added each time being 1 / 3 of the total amount of the conductive graphite powder.
9. Use of the composite conductive particles according to any one of claims 1 to 8 in the recycling of waste lithium batteries.