Ultrasonic strengthening modification and nitriding composite processing device and processing method thereof
By using a combined ultrasonic strengthening and nitriding processing device, along with automatic monitoring and adjustment of ammonia decomposition rate, the problems of thin metal surface strengthening layer thickness and low nitriding efficiency were solved, achieving efficient nitriding treatment and improved fatigue resistance.
Patent Information
- Application Number
- CN202310741266.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-20
AI Technical Summary
The thickness of the reinforced layer of metal after ultrasonic strengthening and modification is not high. Traditional nitriding treatment is complicated and inefficient, the morphology of the nitrided layer is not easy to control, and the processing quality is poor.
An ultrasonic strengthening modification and nitriding composite processing device is adopted, which combines an ultrasonic amplitude transformer, an induction heating ring, an ammonia decomposition rate detector and a system controller to achieve automatic monitoring and adjustment of the ammonia decomposition rate and carry out efficient nitriding treatment.
It improves the thickness and surface morphology of the metal surface strengthening layer, enhances fatigue resistance, achieves efficient nitriding treatment, has a reasonable structural design, is simple to operate, is environmentally friendly and pollution-free, and is highly efficient.
Smart Images

Figure CN116770035B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface processing, in particular to an ultrasonic strengthening modification and nitriding composite processing device and a processing method thereof. Background Art
[0002] According to theoretical research and practical proof, ultrasonic strengthening and modification technology uses abrasive materials to impact the metal surface with high energy density, forming a surface texture morphology of interconnected groove and pocket microstructures, greatly improving the residual compressive stress distribution on the metal surface, thereby increasing the service life of metal parts; nitriding technology is a conventional heat treatment that can produce a strengthening layer of several millimeters on the metal surface.
[0003] However, the thickness of the metal strengthening layer after the existing ultrasonic strengthening modification processing is generally not high, within the range of several hundred microns; traditional gas nitriding needs to rely on manual repeated monitoring of the ammonia decomposition rate during the nitriding process through a burette to control the nitriding layer structure. The operation is complicated and the nitriding efficiency is low. The nitriding layer morphology is difficult to control and the processing quality is poor.
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides an ultrasonic strengthening modification and nitriding composite processing device and a processing method thereof, which can strengthen the metal surface, improve the thickness and surface morphology of its surface strengthening layer, improve its fatigue resistance, and realize high-efficiency nitriding treatment of the metal surface by automatically monitoring and adjusting the ammonia decomposition rate. Summary of the invention
[0005] The object of the present invention is to provide an ultrasonic strengthening modification and nitriding composite processing device and a processing method thereof, by which the metal surface can be strengthened, the thickness of its surface strengthening layer and the surface morphology can be improved, the fatigue resistance can be improved, and the metal surface can be efficiently nitrided by automatically monitoring and adjusting the ammonia decomposition rate.
[0006] On the one hand, the present invention provides an ultrasonic enhanced modification and nitriding composite processing device, comprising: a gas reaction furnace, a processing platform, a processing cavity, an induction heating ring, an ultrasonic horn, an ultrasonic transducer, an ultrasonic generator, an ammonia decomposition rate detector and a system controller;
[0007] The top of the gas reaction furnace is connected to the inside of the processing chamber through a hydrogen delivery pipeline, an ammonia delivery pipeline and a nitrogen delivery pipeline, respectively, for introducing hydrogen, ammonia and nitrogen into the processing chamber, the induction heating ring is arranged on the outside of the processing chamber, and the induction heating ring is placed on the surface of the processing platform, the sample to be processed is arranged in the processing chamber and can be nitrided therein, and the processing chamber is connected to the middle of the gas reaction furnace through a mixed gas receiving pipeline, for inputting the mixed gas generated in the processing chamber into the gas reaction furnace;
[0008] The ultrasonic horn is connected to the bottom of the processing chamber, and can accelerate the abrasive material to make it impact the surface of the sample to be processed at high frequency, thereby achieving surface modification of the sample to be processed;
[0009] The ultrasonic transducer is installed at the bottom end of the ultrasonic horn and can drive the ultrasonic horn through ultrasonic waves;
[0010] The ultrasonic generator is electrically connected to the ultrasonic transducer, and the high-frequency electrical signal provided by the ultrasonic generator can be converted into ultrasonic waves through the ultrasonic transducer;
[0011] The ammonia decomposition rate detector is connected to the mixed gas receiving pipeline through an ammonia decomposition rate detection pipeline, and is used to detect the decomposition rate of ammonia in the mixed gas discharged from the processing chamber;
[0012] The system controller is electrically connected to the ammonia decomposition rate detector and the gas reaction furnace respectively, and controls the emission of each gas in the gas reaction furnace in real time according to the detected ammonia decomposition rate.
[0013] Preferably, a detachable processing chamber end cover is installed on the top of the processing chamber, and a sample carrying platform is provided between the processing chamber and the processing chamber end cover, and the sample to be processed is fixed on the sample carrying platform.
[0014] Preferably, the sample carrier is fixed to the inner side of the end cover of the processing chamber by screw connection, and the sample to be processed is adhered to the surface of the sample carrier by a phosphate-based high-temperature-resistant inorganic adhesive.
[0015] Preferably, the hydrogen delivery pipeline, the ammonia delivery pipeline and the nitrogen delivery pipeline are connected to the side of the processing chamber away from the gas reactor through a cross four-way quick-connect joint, and the side of the processing chamber close to the gas reactor is connected to the mixed gas receiving pipeline through a quick-connect pipeline, and the mixed gas receiving pipeline is connected to the ammonia decomposition rate detection pipeline through a three-way pipeline joint.
[0016] Preferably, one end of the hydrogen delivery pipeline, the ammonia delivery pipeline and the nitrogen delivery pipeline are connected to the top of the gas reaction furnace through a quick-connect pipe female joint and a straight quick-connect joint, and the hydrogen delivery pipeline, the ammonia delivery pipeline and the nitrogen delivery pipeline are respectively connected to a one-way throttle valve, and a first support seat is provided at the bottom of each one-way throttle valve, a second support seat is provided at the bottom of the cross four-way quick-connect joint, and a third support seat is provided at the bottom of the three-way pipe joint, and the bottoms of the first support seat, the second support seat and the third support seat are fixedly connected to the processing platform through connecting bolts.
[0017] Preferably, the ultrasonic amplitude transformer includes an amplitude transformer interface, a rod body and a rod head, the amplitude transformer interface is connected to the ultrasonic transducer, the rod body is used to focus the ultrasonic waves emitted by the ultrasonic transducer to the rod head area, the bottom of the processing cavity is fixed to the surface of the processing platform by a bolt pair, and the bottom end of the processing cavity is adapted to be sealed and connected to the rod head, and the bottom end of the processing cavity is provided with a slope.
[0018] Preferably, the ultrasonic transducer comprises a driving electrode, piezoelectric ceramics and a main body, the driving electrode is connected to the ultrasonic generator via a wire, and the main body is fixedly connected to the ultrasonic horn via bolts.
[0019] Preferably, the gas reaction furnace includes a furnace body, an input interface and three output interfaces, and a gas receiving chamber, an ammonia storage chamber, a hydrogen storage chamber, a nitrogen storage chamber and a gas processor are arranged in the furnace body. The gas processor is used to separate the mixed gas in the gas receiving chamber into ammonia, hydrogen and nitrogen and store them in the ammonia storage chamber, the hydrogen storage chamber and the nitrogen storage chamber respectively. The input interface is connected to the mixed gas receiving pipeline, and the three output interfaces are connected to the ammonia delivery pipeline, the hydrogen delivery pipeline and the nitrogen delivery pipeline respectively. An air pressure sensor is arranged between the input interface and the mixed gas receiving pipeline, and the air pressure sensor is used to monitor the air pressure in the processing chamber.
[0020] Preferably, the system controller is provided with a power switch, a gas pressure setting button, a temperature setting button and a gas flow rate adjustment button, through which the gas flow rate of the input interface and each output interface of the gas reaction furnace can be adjusted to control the gas pressure in the processing chamber to reach the gas pressure range required for nitriding, and the induction heating ring is connected to the system controller through a wire. When the system controller controls the induction heating ring to be energized, the induction heating ring generates eddy currents inside the processing chamber, causing it to heat up rapidly to reach the temperature required for nitriding.
[0021] On the other hand, the present invention provides a method for ultrasonic strengthening modification and nitriding composite processing using an ultrasonic strengthening modification and nitriding composite processing device, comprising the following steps:
[0022] Step 1: Clean and dry the processing cavity, and add suitable abrasives into the processing cavity;
[0023] Step 2: fixing the sample to be processed in the processing chamber and sealing it;
[0024] Step 3: Open the nitrogen delivery pipeline and the mixed gas receiving pipeline to fill the processing chamber with nitrogen atmosphere, so as to reduce oxidation of the sample to be processed when it comes into contact with air during the processing;
[0025] Step 4: Close all the delivery pipelines, turn on the power of the ultrasonic generator, perform ultrasonic strengthening and modification processing on the sample to be processed, and turn off the power of the ultrasonic generator after the processing is completed;
[0026] Step 4: Set the gas pressure Pa, temperature T and ammonia decomposition rate range (η min , η max ), turn on the switch of the system controller to start nitriding;
[0027] Step 5: Open the ammonia delivery pipeline, the mixed gas receiving pipeline and the induction heating ring to fill the processing chamber with ammonia atmosphere and reach the set pressure range Pa and temperature T;
[0028] Step 6: The system controller automatically adjusts the input flow rates of ammonia, hydrogen and nitrogen according to the decomposition rate η measured in real time by the ammonia decomposition rate detector.
[0029] When the measured ammonia decomposition rate η is within η min ≤η≤η max Within the range, ammonia gas continues to be input into the processing chamber;
[0030] When the measured ammonia decomposition rate η is η>η max If the ammonia decomposition rate η is within the set range, the nitrogen delivery pipeline is opened to input nitrogen into the processing chamber until the ammonia decomposition rate η returns to the set range and then the nitrogen delivery pipeline is closed;
[0031] When the measured ammonia decomposition rate η is within η<η min If the ammonia decomposition rate η is within the set range, the hydrogen delivery pipeline is opened to input hydrogen into the processing chamber until the ammonia decomposition rate η recovers to the set range and then the hydrogen delivery pipeline is closed.
[0032] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0033] 1. The present invention generates ultrasonic waves by using an ultrasonic generator and an ultrasonic transducer, and the ultrasonic horn connected to the bottom of the processing cavity contacts the abrasive to give it extremely high kinetic energy, so that it performs high-frequency impact on the metal surface of the sample to be processed in the processing cavity, thereby realizing surface modification processing of the workpiece, and an induction heating ring is arranged outside the processing cavity to heat the sample to be processed in the processing cavity, and nitrogen, ammonia and hydrogen are introduced into the processing cavity in conjunction with a gas reaction furnace and a hydrogen delivery pipeline, an ammonia delivery pipeline and a nitrogen delivery pipeline, so as to perform a nitriding reaction, thereby realizing ultrasonic strengthening modification and nitriding composite processing, thereby improving the thickness and surface morphology of the metal surface strengthening layer and improving its anti-fatigue performance;
[0034] 2. The processing method of first ultrasonic strengthening modification and then nitriding in the present invention can better open the ion channels on the metal surface, allowing active nitrogen atoms to enter the metal more easily, thereby improving the nitriding effect of the metal surface;
[0035] 3. The present invention can monitor and automatically control the ammonia decomposition rate in real time through the ammonia decomposition rate detector and the system controller, thereby ensuring efficient nitriding treatment of the sample to be processed;
[0036] 4. The present invention can recycle the mixed gas generated in the nitriding process into the gas reaction furnace, decompose and separate it, so that it can be recycled in the device, reducing pollution and saving costs;
[0037] 5. The processing device of the present invention has reasonable structural design, simple operation, strong applicability, environmental protection and pollution-free, and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 It is a schematic diagram of the overall structure of the ultrasonic strengthening modification and nitriding composite processing device of the present invention;
[0040] Figure 2 It is a partial cross-sectional view of the ultrasonic strengthening modification and nitriding composite processing device of the present invention;
[0041] Description of reference numerals:
[0042] 1: gas reactor; 2: quick-connect pipe female joint; 3: straight-through quick-connect joint; 4: mixed gas receiving pipeline; 5: three-way pipe joint; 6: third support seat; 7: one-way throttle valve; 8: quick-connect pipe; 9: processing chamber end cover; 10: processing chamber; 11: hydrogen delivery pipeline; 12: ammonia delivery pipeline; 13: induction heating ring; 14: cross four-way quick-connect joint; 15: first support seat; 16: aluminum profile; 17: second support seat; 18: nitrogen delivery pipeline; 19: ultrasonic amplitude transformer; 20: ultrasonic transducer; 21: wire; 22: processing platform; 23: ultrasonic generator; 24: ammonia decomposition rate detection pipeline; 25: ammonia decomposition rate detector; 26: system controller; 27: sample carrier; 28: sample to be processed. DETAILED DESCRIPTION
[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0045] In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined. In addition, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0046] like Figure 1 ,2 As shown, the present invention provides an ultrasonic strengthening modification and nitriding composite processing device, comprising: a gas reaction furnace 1, a processing platform 22, a processing cavity 10, an induction heating ring 13, an ultrasonic horn 19, an ultrasonic transducer 20, an ultrasonic generator 23, an ammonia decomposition rate detector 25 and a system controller 26;
[0047] The top of the gas reactor 1 is connected to the inside of the processing chamber 10 through a hydrogen delivery pipeline 11, an ammonia delivery pipeline 12 and a nitrogen delivery pipeline 18, respectively, for introducing hydrogen, ammonia and nitrogen into the processing chamber 10. The induction heating ring 13 is arranged on the outside of the bottom of the processing chamber 10, and the induction heating ring 13 is placed on the surface of the processing platform 22, which can quickly make the processing chamber 10 reach a high-temperature working condition to meet the nitriding conditions; the inside of the processing chamber 10 is a sealed space, and the sample 28 to be processed is arranged in the processing chamber 10. The processing chamber 10 can provide a closed working space for ultrasonic strengthening modification processing and nitriding treatment, and the processing chamber 10 is connected to the middle of the gas reactor 1 through a mixed gas receiving pipeline 4, which is used to input the mixed gas generated after the nitriding reaction of the processing chamber 10 into the gas reactor 1 for recovery, separation and reuse;
[0048] The ultrasonic horn 19 is connected to the bottom of the processing chamber 10, and the head of the ultrasonic horn 19 is in contact with the abrasive in the processing chamber 10, giving it extremely high kinetic energy, so that it accelerates and impacts the surface of the sample to be processed with high frequency, thereby achieving modification processing on the surface of the sample to be processed;
[0049] The ultrasonic transducer 20 is installed at the bottom end of the ultrasonic horn 19, and is capable of generating ultrasonic waves for driving the ultrasonic horn 19, and is the direct power source of the ultrasonic horn 19;
[0050] The ultrasonic generator 23 is electrically connected to the ultrasonic transducer. The high-frequency electrical signal provided by the ultrasonic generator 23 can be converted into ultrasonic waves through the ultrasonic transducer 20, which is an indirect power source for the ultrasonic horn 19.
[0051] The ammonia decomposition rate detector 25 is connected to the mixed gas receiving pipeline 4 through the ammonia decomposition rate detection pipeline 24. The mixed gas generated after the nitriding reaction in the processing chamber 10 is diverted through the ammonia decomposition rate detection pipeline 24 and then input into the ammonia decomposition rate detector 25, thereby detecting the decomposition rate of ammonia in the mixed gas discharged from the processing chamber 10;
[0052] The system controller 26 is electrically connected to the ammonia decomposition rate detector 25 and the gas reaction furnace 1 through the wire 21, and can control the emission of each gas in the gas reaction furnace 1 in real time according to the detected ammonia decomposition rate.
[0053] Specifically, a detachable processing chamber end cover 9 is installed on the top of the processing chamber 10, and the processing chamber end cover 9 is sealed and connected to the processing chamber 10 through multiple screws. The bottom of the processing chamber 10 is fixedly connected to the processing platform 22 through ear plates and screws. A sample carrier 27 is provided between the processing chamber 10 and the processing chamber end cover 9, and the sample 28 to be processed is fixed on the sample carrier 27. In this embodiment, the sample carrier 27 is fixed to the inner side of the processing chamber end cover 9 by screw connection, and the sample 28 to be processed is adhered to the bottom surface of the sample carrier 27 by a phosphate-based high-temperature resistant inorganic adhesive, which meets the high-temperature working conditions required for the nitriding reaction. A slope is provided at the lower end of the processing chamber 10, so that the abrasive quickly returns to the bottom of the processing chamber 10 after hitting the sample 28 to be processed, thereby improving the processing efficiency of the abrasive.
[0054] Interfaces are provided on both sides of the processing chamber 10 (i.e., the side close to the gas reactor 1 and the side away from it), and one end of the hydrogen delivery pipeline 11, the ammonia delivery pipeline 12 and the nitrogen delivery pipeline 18 are connected to the top of the gas reactor 1 through the quick-connect pipeline female joint 2 and the straight-through quick-connect joint 3, and the other ends of the hydrogen delivery pipeline 11, the ammonia delivery pipeline 12 and the nitrogen delivery pipeline 18 are simultaneously connected to the interface of the processing chamber 10 away from the gas reactor 1 through the cross four-way quick-connect joint 14, which are respectively used to transport the ammonia, hydrogen and nitrogen in the gas reactor 1 to the processing chamber 10, and cooperate with the sense of The processing chamber 10 is heated to a high temperature by the heating ring 13, and the interface of the processing chamber 10 on the side close to the gas reactor 1 is connected to the mixed gas receiving pipe 4 through the quick-connect pipe 8. The mixed gas receiving pipe 4 is connected to the ammonia decomposition rate detection pipe 24 through the three-way pipe joint 5. The reacted mixed gas flows out of the processing chamber 10 and flows back to the gas reactor 1 through the quick-connect pipe 8 and the mixed gas receiving pipe 4 for recovery, separation and storage. Part of the mixed gas can be diverted through the ammonia decomposition rate detection pipe 24, and the mixed gas can be detected by the ammonia decomposition rate detector 25 to detect the decomposition rate of the ammonia.
[0055] The hydrogen delivery pipeline 11, the ammonia delivery pipeline 12 and the nitrogen delivery pipeline 18 are respectively connected with a one-way throttle valve 7. Each one-way throttle valve 7 plays a role in controlling the flow direction of the gas in each delivery pipeline to prevent the gas from flowing back during the delivery process, thereby causing measurement errors or even control failure. A first support seat 15 is provided at the bottom of each one-way throttle valve 7, a second support seat 17 is provided at the bottom of the cross four-way quick-connect joint 14, and a third support seat 6 is provided at the bottom of the three-way pipe joint 5. The first support seat 15, the second support seat 17 and the third support seat 6 are all U-shaped, and one end of each of them is provided with a rib extending to both sides. The rib is fixedly connected to the surface of the processing platform 22 by connecting bolts. By supporting the one-way throttle valve 7, the cross four-way quick-connect joint 14 and the three-way pipe joint 5, it is ensured that they can be normally connected to each pipeline, and the pipeline deformation caused by their weight is prevented, so as to ensure their normal operation.
[0056] Specifically, the ultrasonic amplitude transformer 19 includes an amplitude transformer interface, a rod body and a rod head, and can be connected to the ultrasonic transducer 20 at the bottom thereof through the amplitude transformer interface. The rod body is used to focus the ultrasonic waves emitted by the ultrasonic transducer 20 to the rod head area. The bottom of the processing cavity 10 is fixed to the surface of the processing platform 22 by a bolt pair, and the bottom end of the processing cavity 22 is adapted and sealed to the rod head. A slope is provided at the bottom end of the processing cavity 10. The ultrasonic waves focused by the rod head can generate extremely high kinetic energy for the abrasive in contact with it, so that it is accelerated and then subjected to high-frequency impact on the surface of the sample 28 to be processed, thereby realizing modification processing on the surface of the sample 28 to be processed.
[0057] Specifically, the ultrasonic transducer 20 includes a driving electrode, a piezoelectric ceramic and a main body, wherein the driving electrode is connected to the ultrasonic generator 23 through a wire 21, and the main body is fixedly connected to the horn interface of the ultrasonic horn 19 through a bolt. The ultrasonic generator 23 is provided with a power switch, a frequency adjustment key and a wire 21, wherein the wire 21 is connected to the ultrasonic transducer 20.
[0058] In this embodiment, the gas reaction furnace 1 includes a furnace body, an input interface and three output interfaces. A gas receiving chamber, an ammonia storage chamber, a hydrogen storage chamber, a nitrogen storage chamber and a gas processor are arranged in the furnace body. The ammonia storage chamber, the hydrogen storage chamber and the nitrogen storage chamber are respectively connected to the ammonia delivery pipeline 12, the hydrogen delivery pipeline 11 and the nitrogen delivery pipeline 18 through three output interfaces, so as to introduce ammonia, hydrogen and nitrogen into the processing chamber 10. The gas processor is used to separate the mixed gas in the gas receiving chamber into ammonia, hydrogen and nitrogen, and store them in the ammonia storage chamber, the hydrogen storage chamber and the nitrogen storage chamber respectively. The input interface is connected to the mixed gas receiving pipeline 4. An air pressure sensor is arranged between the input interface and the mixed gas receiving pipeline 4. The air pressure sensor is used to monitor the air pressure in the processing chamber 10.
[0059] The system controller 26 is provided with a power switch, an air pressure setting button, a temperature setting button and a gas flow rate adjustment button. According to the air pressure in the processing chamber 10 measured by the air pressure sensor, the gas flow rate of the input interface and each output interface of the gas reaction furnace 1 is adjusted through the gas flow rate adjustment button to control the gas supply during the nitriding treatment of the processing chamber 10, so that the air pressure reaches the air pressure range required for nitriding. The induction heating ring 13 is also connected to the system controller 26 through a wire. When the system controller 26 controls the induction heating ring 13 to be energized, the induction heating ring 13 generates eddy currents inside the processing chamber 10, causing it to heat up quickly to reach the temperature required for nitriding.
[0060] The ammonia decomposition rate detector 25 is provided with a gas detection interface, a power switch, and a decomposition rate adjustment key, wherein the gas detection interface is connected to the ammonia decomposition rate detection pipeline 24 through the quick-connect pipeline female connector 2, and is used to monitor the decomposition rate of ammonia in the processing cavity 10 in real time and provide timely feedback to the system controller 26.
[0061] Four aluminum profiles 16 are installed at the bottom of the processing platform 22 to support the processing platform 22 , and the aluminum profiles 16 and the processing platform 22 are connected by screws.
[0062] On the other hand, the present invention also provides a method for ultrasonic strengthening modification and nitriding composite processing using the above device, which specifically includes the following steps:
[0063] Step 1: Open the processing chamber end cover 9, clean and dry the processing chamber 10, and select appropriate abrasives and add them into the processing chamber 10;
[0064] Step 2: The sample 28 to be processed is fixed on the surface of the sample support table 27 by using a phosphate-based high temperature resistant inorganic adhesive, and the processing chamber end cover 9 and the processing chamber body 10 are sealed by screws;
[0065] Step 3: Open the nitrogen delivery pipeline 18 and the mixed gas receiving pipeline 4 to fill the processing chamber 10 with a nitrogen atmosphere, which can effectively reduce oxidation of the sample 28 to be processed when it comes into contact with air during the processing;
[0066] Step 4: Close all the conveying pipelines, turn on the power of the ultrasonic generator 23, and convert the high-frequency electrical signal of the ultrasonic generator 23 into ultrasonic waves for driving the ultrasonic horn 19 through the ultrasonic transducer 20, so as to give extremely high kinetic energy to the abrasive in the processing cavity 10, so that it impacts the metal surface with high frequency, thereby performing ultrasonic strengthening and modification processing on the sample 28 to be processed. After the processing is completed, turn off the power of the ultrasonic generator 23;
[0067] Step 4: Set the gas pressure Pa, temperature T and ammonia decomposition rate range (η min , η max), turn on the switch of the system controller 26 to start nitriding;
[0068] Step 5: Open the ammonia gas delivery pipeline 12, the mixed gas receiving pipeline 4 and the induction heating ring 13, so that the processing chamber 10 is filled with an ammonia atmosphere and reaches the set pressure range Pa and temperature T;
[0069] Step 6: The system controller 26 automatically adjusts the input flow rates of ammonia, hydrogen and nitrogen according to the decomposition rate η measured in real time by the ammonia decomposition rate detector 25, according to the decomposition of ammonia into hydrogen and nitrogen under high temperature and high pressure conditions, that is,
[0070]
[0071] By increasing the concentration of nitrogen to reduce the decomposition rate of ammonia and increasing the concentration of hydrogen to increase the decomposition rate of ammonia, the decomposition rate of ammonia during the nitriding process can be adjusted to achieve a more efficient nitriding effect. The specific control is as follows:
[0072] When the measured ammonia decomposition rate η is within η min ≤η≤η max If the ammonia gas is within the range, the ammonia gas is continuously introduced into the processing chamber 10 to improve the nitriding effect;
[0073] When the measured ammonia decomposition rate η is η>η max If the ammonia decomposition rate η is within the set range, the nitrogen delivery pipeline 18 is opened to input nitrogen into the processing chamber 10 until the ammonia decomposition rate η returns to the set range and then the nitrogen delivery pipeline 18 is closed;
[0074] When the measured ammonia decomposition rate η is within η<η min If the ammonia decomposition rate η is within the set range, the hydrogen delivery pipeline 11 is opened to input hydrogen into the processing chamber 10, and then the hydrogen delivery pipeline 11 is closed until the ammonia decomposition rate η returns to the set range.
[0075] The processing method of first ultrasonic strengthening modification and then nitriding adopted in the present invention can better open the ion channels on the metal surface, allowing active nitrogen atoms to more easily enter the interior of the metal, thereby improving the nitriding effect of the metal surface, and the ammonia decomposition rate is monitored in real time by the ammonia decomposition rate detector 25, and the opening and closing and flow rate of each conveying pipeline are automatically controlled by the system controller 26 in the above manner, and the input gas is controlled to keep the ammonia decomposition rate within an appropriate range, thereby ensuring efficient nitriding treatment of the sample 28 to be processed.
[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An ultrasonic strengthening modification and nitriding composite processing device, characterized in that: include: Gas reaction furnace, processing platform, processing chamber, induction heating ring, ultrasonic horn, ultrasonic transducer, ultrasonic generator, ammonia decomposition rate detector and system controller; The top of the gas reaction furnace is connected to the inside of the processing chamber through a hydrogen delivery pipeline, an ammonia delivery pipeline and a nitrogen delivery pipeline, respectively, for introducing hydrogen, ammonia and nitrogen into the processing chamber, the induction heating ring is arranged on the outside of the processing chamber, and the induction heating ring is placed on the surface of the processing platform, the sample to be processed is arranged in the processing chamber and can be nitrided therein, and the processing chamber is connected to the middle of the gas reaction furnace through a mixed gas receiving pipeline, for inputting the mixed gas generated in the processing chamber into the gas reaction furnace; The ultrasonic horn is connected to the bottom of the processing chamber, and can accelerate the abrasive material to make it impact the surface of the sample to be processed at high frequency, thereby achieving surface modification of the sample to be processed; The ultrasonic transducer is installed at the bottom end of the ultrasonic horn and can drive the ultrasonic horn through ultrasonic waves; The ultrasonic generator is electrically connected to the ultrasonic transducer, and the high-frequency electrical signal provided by the ultrasonic generator can be converted into ultrasonic waves through the ultrasonic transducer; The ammonia decomposition rate detector is connected to the mixed gas receiving pipeline through an ammonia decomposition rate detection pipeline, and is used to detect the decomposition rate of ammonia in the mixed gas discharged from the processing chamber; The system controller is electrically connected to the ammonia decomposition rate detector and the gas reaction furnace respectively, and controls the emission of each gas in the gas reaction furnace in real time according to the detected ammonia decomposition rate.
2. The ultrasonic strengthening modification and nitriding composite processing device according to claim 1 is characterized in that: A detachable processing chamber end cover is installed on the top of the processing chamber body, and a sample carrying platform is arranged between the processing chamber body and the processing chamber end cover, and the sample to be processed is fixed on the sample carrying platform.
3. The ultrasonic strengthening modification and nitriding composite processing device according to claim 2 is characterized in that: The sample carrier is fixed to the inner side of the processing chamber end cover by screw connection, and the sample to be processed is adhered to the surface of the sample carrier by a phosphate-based high-temperature-resistant inorganic adhesive.
4. The ultrasonic strengthening modification and nitriding composite processing device according to claim 2 is characterized in that: The hydrogen delivery pipeline, the ammonia delivery pipeline and the nitrogen delivery pipeline are connected to the side of the processing chamber away from the gas reaction furnace through a cross four-way quick-connect joint, and the side of the processing chamber close to the gas reaction furnace is connected to the mixed gas receiving pipeline through a quick-connect pipeline, and the mixed gas receiving pipeline is connected to the ammonia decomposition rate detection pipeline through a three-way pipeline joint.
5. The ultrasonic strengthening modification and nitriding composite processing device according to claim 4 is characterized in that: One ends of the hydrogen delivery pipeline, the ammonia delivery pipeline and the nitrogen delivery pipeline are connected to the top of the gas reaction furnace through a quick-connect pipeline female joint and a straight quick-connect joint. The hydrogen delivery pipeline, the ammonia delivery pipeline and the nitrogen delivery pipeline are respectively connected to a one-way throttle valve, and a first support seat is provided at the bottom of each one-way throttle valve, a second support seat is provided at the bottom of the cross four-way quick-connect joint, and a third support seat is provided at the bottom of the three-way pipeline joint. The bottoms of the first support seat, the second support seat and the third support seat are fixedly connected to the processing platform through connecting bolts.
6. The ultrasonic strengthening modification and nitriding composite processing device according to claim 1 is characterized in that: The ultrasonic amplitude transformer includes an amplitude transformer interface, a rod body and a rod head, the amplitude transformer interface is connected to the ultrasonic transducer, the rod body is used to focus the ultrasonic waves emitted by the ultrasonic transducer to the rod head area, the bottom of the processing cavity is fixed to the surface of the processing platform by a bolt pair, and the bottom end of the processing cavity is adapted to be sealed and connected to the rod head, and the bottom end of the processing cavity is provided with a slope.
7. The ultrasonic strengthening modification and nitriding composite processing device according to claim 1 is characterized in that: The ultrasonic transducer comprises a driving electrode, piezoelectric ceramics and a main body. The driving electrode is connected to the ultrasonic generator via a wire, and the main body is fixedly connected to the ultrasonic horn via bolts.
8. The ultrasonic strengthening modification and nitriding composite processing device according to claim 1 is characterized in that: The gas reaction furnace includes a furnace body, an input interface and three output interfaces. A gas receiving chamber, an ammonia storage chamber, a hydrogen storage chamber, a nitrogen storage chamber and a gas processor are arranged in the furnace body. The gas processor is used to separate the mixed gas in the gas receiving chamber into ammonia, hydrogen and nitrogen and store them in the ammonia storage chamber, the hydrogen storage chamber and the nitrogen storage chamber respectively. The input interface is connected to the mixed gas receiving pipeline, and the three output interfaces are connected to the ammonia delivery pipeline, the hydrogen delivery pipeline and the nitrogen delivery pipeline respectively. An air pressure sensor is arranged between the input interface and the mixed gas receiving pipeline, and the air pressure sensor is used to monitor the air pressure in the processing chamber.
9. The ultrasonic strengthening modification and nitriding composite processing device according to claim 8, characterized in that: The system controller is provided with a power switch, a gas pressure setting button, a temperature setting button and a gas flow rate adjustment button. The gas flow rate adjustment button can be used to adjust the gas flow rate of the input interface and each output interface of the gas reaction furnace to control the gas pressure in the processing chamber to reach the gas pressure range required for nitriding. The induction heating ring is connected to the system controller through a wire. When the system controller controls the induction heating ring to be energized, the induction heating ring generates eddy currents inside the processing chamber to quickly heat it up to reach the temperature required for nitriding.
10. A method for performing ultrasonic strengthening modification and nitriding composite processing using the ultrasonic strengthening modification and nitriding composite processing device according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: Clean and dry the processing cavity, and add suitable abrasives into the processing cavity; Step 2: fixing the sample to be processed in the processing chamber and sealing it; Step 3: Open the nitrogen delivery pipeline and the mixed gas receiving pipeline to fill the processing chamber with nitrogen atmosphere, so as to reduce oxidation of the sample to be processed when it comes into contact with air during the processing; Step 4: Close all the delivery pipelines, turn on the power of the ultrasonic generator, perform ultrasonic strengthening and modification processing on the sample to be processed, and turn off the power of the ultrasonic generator after the processing is completed; Step 4: Set the gas pressure Pa, temperature T and ammonia decomposition rate range (η min , η max ), turn on the switch of the system controller to start nitriding; Step 5: Open the ammonia delivery pipeline, the mixed gas receiving pipeline and the induction heating ring to fill the processing chamber with ammonia atmosphere and reach the set pressure range Pa and temperature T; Step 6: The system controller automatically adjusts the input flow rates of ammonia, hydrogen and nitrogen according to the decomposition rate η measured in real time by the ammonia decomposition rate detector. When the measured ammonia decomposition rate η is within η min ≤η≤η max Within the range, ammonia gas continues to be input into the processing chamber; When the measured ammonia decomposition rate η is η>η max If the ammonia decomposition rate η is within the set range, the nitrogen delivery pipeline is opened to input nitrogen into the processing chamber until the ammonia decomposition rate η returns to the set range and then the nitrogen delivery pipeline is closed; When the measured ammonia decomposition rate η is within η<η min If the ammonia decomposition rate η is within the set range, the hydrogen delivery pipeline is opened to input hydrogen into the processing chamber until the ammonia decomposition rate η recovers to the set range and then the hydrogen delivery pipeline is closed.