A kind of low carbon tailings concrete and preparation method thereof
By using modified straw fibers and high-temperature calcined bauxite tailings powder in tailings concrete, combined with triisopropanolamine, the problem of insufficient mechanical properties and impermeability resistance of tailings concrete is solved, and a higher Building strength and environmental protection effect.
Patent Information
- Application Number
- CN202310854943.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-07-13
AI Technical Summary
The mechanical properties and permeability of tailings concrete are difficult to meet the requirements, resulting in shortcomings in construction applications.
Use low-carbon tailings concrete formula, including 70-80% cement, 300-410 parts of gravel, 100-135 parts of iron tailings sand, 150-210 parts of bauxite tailings powder, 10-15 parts of triisopropanolamine and 20-35 parts of modified straw fibers, and the modified straw fibers are coated with high temperature calcination and polyethylene glycol to improve the binding force of tailings and cement colloids, and the fluidity and permeability of concrete.
It significantly improves the mechanical properties and permeability of low-carbon tailings concrete, meets the strength requirements of building materials, and reduces the amount of cement, reduces carbon emissions and environmental pollution.
Smart Images

Figure BDA0004335604290000061 
Figure BDA0004335604290000081 
Figure BDA0004335604290000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to low-carbon tailings concrete and a preparation method thereof. Background Art
[0002] With the accelerated development of urbanization in my country, the demand for building materials has increased dramatically. The large-scale exploitation of natural resources such as natural sand and gravel has seriously damaged the ecological environment. Moreover, these resources are non-renewable in the short term, making the contradiction of shortage of building resources increasingly prominent. Therefore, it is urgent to find suitable alternative materials.
[0003] Tailings are solid wastes discharged by mining enterprises in the process of refining the main raw materials for metallurgy. my country discharges a large amount of tailings solid wastes every year. Tailings or tailings have become the solid wastes with the largest output and the largest stockpile in my country. The large stockpile of tailings not only pollutes the environment, but also occupies land resources. Applying mine tailings to the field of concrete production technology can not only make the mines with exhausted or insufficient resources become new resource bases to resume and expand production, but also open up the scientific and technological fields of new materials and promote technological progress. At the same time, it is also conducive to alleviating environmental pollution and improving the ecological environment.
[0004] Therefore, using tailings as admixtures in concrete can, on the one hand, replace natural sand and gravel to alleviate the increasingly scarce status of natural sand resources, and on the other hand, it can partially replace cement for concrete construction. It is one of the methods that can be considered for the reuse of mine tailings. Using mine tailings instead of cement to produce concrete has many advantages, such as preventing the release of heavy metals, solving the problem of tailings occupying space, and preventing pollutants from infiltrating the environment. In addition, the use of tailings reduces the demand for cement. It can reduce carbon emissions and reduce the pollution of solid waste to the ecological environment, which has great practical significance.
[0005] Although using tailings as concrete mineral admixtures can effectively utilize tailings, due to the large differences in the mineral composition of tailings, the activity of tailings directly added to concrete is low and cannot play a better skeleton role, resulting in the mechanical properties and impermeability of the resulting concrete being difficult to meet the requirements. Summary of the invention
[0006] In order to significantly improve the mechanical properties and impermeability of tailings concrete and greatly increase the comprehensive utilization rate of tailings concrete, the present application provides a low-carbon tailings concrete and a preparation method thereof.
[0007] The present application provides a low-carbon tailings concrete, which adopts the following technical solution:
[0008] A low-carbon tailings concrete comprises the following raw materials in parts by weight:
[0009] 70-80 parts of cement;
[0010] 300-410 parts of crushed stone;
[0011] Iron tailings 100-135 parts;
[0012] Bauxite tailings powder 150-210 parts;
[0013] 10-15 parts of triisopropanolamine;
[0014] 20-35 parts of modified straw fiber;
[0015] 35-55 parts water;
[0016] The bauxite tailing powder is obtained by subjecting the bauxite tailing coarse material to a high-temperature calcination treatment of 450-580° C. The modified straw fiber is modified by coating with polyethylene glycol, and the molecular weight of the polyethylene glycol is 6000-10000.
[0017] By adopting the above technical scheme, the concrete prepared by the present application can effectively utilize tailings and alleviate the contradiction between the increasing shortage of natural river sand and the increasing demand due to the addition of a large amount of abandoned tailings, waste rocks and iron tailings sand. However, compared with natural sand, iron tailings sand is not like river sand in granular structure, with many internal defects, large specific surface area, coarse particles, small fineness, and many edges and corners. In addition, the tailings also contain a certain amount of stone powder, which increases the water demand for mixing concrete and has a certain effect on the fluidity of concrete. Due to the excessive amount of tailings added, the water retention is not as good as natural sand and gravel, the workability is poor, and there is water seepage, which directly affects the fluidity, strength and durability of concrete. Straw fiber is added to concrete as a low-cost, green and low-carbon reinforcing material, which can not only broaden the treatment methods of rural straw, but also reduce the production cost of fiber concrete. At the same time, straw fiber has strong toughness and improves the mechanical properties of concrete. The present application improves the interfacial bonding force between the straw fiber and the cement colloid by modifying the straw fiber and coating the surface of the straw fiber with a layer of polyethylene glycol film. Since polyethylene glycol has a certain water solubility, during the cement mixing process, the polyethylene glycol on the surface of the straw fiber will soften and dissolve to a certain extent, and the dissolved polyethylene glycol will adhere to the surface of the tailings and the cement colloid, thereby enhancing the interfacial bonding between the tailings and the cement colloid, improving the workability and fluidity of the concrete, and improving the mechanical properties of the concrete. In addition, the polyethylene glycol will adhere to the concrete matrix to form a coating film, reduce the contact between the concrete and water, and improve the later stage of the concrete's anti-seepage performance.
[0018] By subjecting the added bauxite tailings powder to high-temperature calcination treatment, the structural water of diaspore and kaolinite in the bauxite tailings powder is completely removed between 450-580°C. As the calcination temperature increases, the aluminosilicate minerals are gradually dehydrated and decomposed, the particle size distribution of the bauxite tailings powder becomes more concentrated, the specific surface area gradually increases, and the activity is improved. It cooperates with the iron tailings to reduce the amount of cement added.
[0019] Optionally, the preparation method of the modified straw fiber includes the following steps: crushing the straw fiber, soaking it in a sodium hydroxide solution, then washing the soaking solution with water until it is neutral, and drying to obtain an initial dry product; then adding a polyethylene glycol solution to the initial dry product, heating the reaction, and drying to obtain the modified straw fiber.
[0020] By adopting the above technical scheme, the straw fiber is first immersed in a sodium hydroxide solution to roughen the surface of the straw fiber, and then mixed with polyethylene glycol. The polyethylene glycol molecules form hydrogen bonds with the straw fiber, and the polyethylene glycol is coated on the surface of the straw fiber, and a layer of polyethylene glycol film is coated on the surface of the straw fiber.
[0021] Optionally, the mass concentration of the sodium hydroxide solution is 3-6wt%.
[0022] By adopting the above technical solution, after the straw fiber is soaked in the sodium hydroxide solution, the roughness of the straw fiber surface is improved and the specific surface area is increased, which is more conducive to the polyethylene glycol being coated on the surface of the straw fiber to form a coating film.
[0023] Optionally, the mass concentration of the polyethylene glycol solution is 7-11 wt %.
[0024] By adopting the above technical scheme, the mass concentration of the polyethylene glycol solution affects whether a coating film can be formed on the surface of the straw fiber. When the mass concentration of the polyethylene glycol is low, the coating amount on the surface of the straw fiber is low. When the mass concentration of the polyethylene glycol is high, the coating amount on the surface of the straw fiber is high, which increases the concentration of the polyethylene glycol added to the concrete and causes a decrease in the early strength of the concrete.
[0025] Optionally, the iron tailings sand has a silicon dioxide mass fraction of 27-30%, a aluminum oxide mass fraction of 8-11%, and a calcium oxide mass fraction of 20-25%.
[0026] By adopting the above technical solution, iron tailings are the waste slag discharged after the iron concentrate is selected by the ore dressing plant. It is one of the main industrial solid wastes. The main mineral composition of iron tailings is silicate minerals such as quartz, feldspar, amphibole and pyroxene. The main chemical composition of iron tailings is SiO 2 、Al 2 O 3 , Fe 2 O3 , CaO and MgO, etc. By selecting iron tailings powder with a certain chemical composition, it contains a higher content of SiO 2 、Al 2 O 3 And CaO, similar to the chemical composition of cement, can replace some traditional cementitious materials and be used as silicon and aluminum raw materials to prepare concrete. The strength of the prepared concrete can meet the use strength of building materials.
[0027] Optionally, the mass fraction of aluminum oxide in the bauxite tailings powder is 40-45%, and the mass fraction of silicon dioxide is 30-37%.
[0028] By adopting the above technical solution, the main chemical composition of bauxite tailings powder is SiO 2 and Al 2 O 3 The mineral contains a certain amount of kaolinite, which can meet the raw material requirements of alkali-activated cementitious materials to a certain extent. The activity of bauxite tailings powder depends on Al 2 O 3 and SiO 2 The mass fraction of Al 2 O 3 、SiO 2 , the formation of gel during the cement hydration process can reduce the amount of cement used and improve the strength of concrete.
[0029] Optionally, the calcination time of the bauxite tailings powder is 30-45 minutes.
[0030] By adopting the above technical scheme, the bauxite tailings powder itself has no activity before calcination and cannot be directly used as a cement-based admixture. Through calcination treatment, the clay minerals in the bauxite tailings powder can be converted into metastable aluminosilicate minerals. As the calcination time increases, the connection and coordination of its stable silicon oxygen tetrahedron and aluminum oxygen octahedron structures will undergo significant changes, and the tetrahedron and octahedron co-vertex connections will separate to form an amorphous aluminum oxygen octahedron structure. This structure has broken bonds and activation points to form metakaolin, which has a higher volcanic ash activity under proper excitation and thus has a higher hydration activity.
[0031] Optionally, the iron tailings sand also includes an activation treatment step before use, and the activation treatment includes the following steps: mixing the iron tailings coarse material and desulfurization gypsum and then grinding them to obtain activated iron tailings powder, and then treating the activated iron tailings powder to obtain iron tailings sand, wherein the mass fraction of the desulfurization gypsum in the iron tailings coarse material is 0.5-0.9wt%.
[0032] By adopting the above technical scheme, in order to improve the activity of iron tailings, desulfurized gypsum is used to grind the coarse iron tailings, which can effectively control the aggregation between particles, weaken the agglomeration effect, and improve the grinding efficiency of the coarse iron tailings. The particle size of the iron tailings powder after grinding is uniform, which changes the crystal structure of the iron tailings, stores a large amount of energy inside, and improves the activity.
[0033] Optionally, the particle size of the bauxite tailings powder is 6-10 μm.
[0034] Optionally, the crushed stone is iron ore tailings waste rock, and the particle size of the iron ore tailings waste rock is 7-20 mm.
[0035] In a second aspect, the present application provides a method for preparing low-carbon tailings concrete, which adopts the following technical solution:
[0036] A method for preparing low-carbon tailings concrete comprises the following steps:
[0037] The crushed stone, iron tailings sand, bauxite tailings powder and triisopropanolamine are mixed evenly, and then cement, water and the modified straw fiber are added and stirred evenly to obtain concrete.
[0038] By adopting the above technical scheme, iron tailings waste rock is used to replace concrete coarse aggregate, iron tailings sand is used to replace fine aggregate, and iron tailings waste rock and bauxite tailings powder are used as silicon and aluminum raw materials. Under the alkaline excitation of triisopropanolamine, silicate gel is generated. These gels can replace part of the cement. At the same time, triisopropanolamine molecules are adsorbed on the surface of concrete to form a layer of charged hydrophilic film, which hinders the coagulation of cement particles, makes cement particles more perfectly contact with water, and accelerates the wetting and penetration of water into cement particles. The modified straw fiber improves the defect of reduced mechanical properties of concrete caused by the addition of tailings.
[0039] In summary, this application has the following beneficial effects:
[0040] 1. In the present application, modified straw fiber is preferably used, and a layer of polyethylene glycol film is coated on the surface of the straw fiber. During the cement mixing process, the polyethylene glycol on the surface of the straw fiber will soften and dissolve to a certain extent, and the dissolved polyethylene glycol will adhere to the surface of the tailings and cement colloid, thereby improving the interfacial bonding force between the straw fiber and the cement colloid, enhancing the interfacial bonding between the tailings powder and the cement colloid, improving the workability and fluidity of the concrete, and improving the mechanical properties of the concrete.
[0041] 2. In this application, the clay minerals in the bauxite tailings powder can be converted into metastable aluminosilicate minerals by calcining the bauxite tailings powder. As the calcination time increases, kaolin is formed. Under proper stimulation, it has higher volcanic ash activity and thus higher hydration activity. It can be compounded with iron tailings waste rock to reduce the amount of cement. DETAILED DESCRIPTION
[0042] The present application is further described in detail below with reference to the embodiments.
[0043] Sources of raw materials: iron tailings, Shaanxi Daxigou Mining Company; bauxite tailings, Shaanxi Dongyixiang Tailings Comprehensive Utilization Co., Ltd., and raw materials used in other embodiments and comparative examples can be derived from common commercial sources unless otherwise specified.
[0044] Preparation example of modified straw fiber
[0045] Preparation Example 1
[0046] The corn straw fiber is placed in a sodium hydroxide aqueous solution with a mass fraction of 5wt%, soaked for 30 minutes, washed with an 8wt% hydrochloric acid aqueous solution until neutral, dried at 60°C, and then placed in a polyethylene glycol aqueous solution with a concentration of 9wt% and a temperature of 60°C, soaked and stirred for 30 minutes, taken out and cooled, and dried at room temperature to obtain modified straw fiber, wherein the molecular weight of the polyethylene glycol is 8000.
[0047] Preparation Example 2
[0048] The difference from Preparation Example 1 is that the mass concentration of the sodium hydroxide aqueous solution is 3wt%, the mass concentration of the polyethylene glycol aqueous solution is 7wt%, and the molecular weight of the polyethylene glycol is 6000.
[0049] Preparation Example 3
[0050] The difference from Preparation Example 1 is that the mass concentration of the sodium hydroxide aqueous solution is 6wt%, the mass concentration of the polyethylene glycol aqueous solution is 11wt%, and the molecular weight of the polyethylene glycol is 10000.
[0051] Preparation Example 4
[0052] The difference from Preparation Example 1 is that the mass concentration of the polyethylene glycol aqueous solution is 7 wt %.
[0053] Preparation Example 5
[0054] The difference from Preparation Example 1 is that the mass concentration of the polyethylene glycol aqueous solution is 11 wt %.
[0055] Preparation Example 6
[0056] The difference from Preparation Example 2 is that the mass concentration of the polyethylene glycol aqueous solution is 3 wt %.
[0057] Preparation Example 7
[0058] The difference from Preparation Example 3 is that the mass concentration of the polyethylene glycol aqueous solution is 15 wt %.
[0059] Preparation Example 8
[0060] The difference from Preparation Example 1 is that the modified straw fiber does not undergo the soaking treatment step in sodium hydroxide solution during the preparation process. The specific preparation steps are as follows: the corn straw fiber is placed in a polyethylene glycol aqueous solution with a concentration of 9wt% and a temperature of 60°C, soaked and stirred for 30 minutes, taken out and cooled, and dried at room temperature to obtain the modified straw fiber.
[0061] Preparation Example 9
[0062] The difference from Preparation Example 1 is that the modified straw fiber is not heated during the immersion in the polyethylene glycol solution. The specific preparation steps are as follows: the corn straw fiber is placed in a 5wt% sodium hydroxide aqueous solution and soaked for 30 minutes. After soaking, it is washed with an 8wt% hydrochloric acid aqueous solution until neutral, dried at 60°C, and then placed in a 9wt% polyethylene glycol aqueous solution, soaked and stirred for 30 minutes, taken out and cooled, and dried at room temperature to obtain the modified straw fiber.
[0063] Preparation Example 10
[0064] The difference from Preparation Example 2 is that the molecular weight of polyethylene glycol is 2,000.
[0065] Preparation Example 11
[0066] The difference from Preparation Example 3 is that the molecular weight of polyethylene glycol is 20,000.
[0067] Example
[0068] Example 1
[0069] A method for preparing low-carbon tailings concrete comprises the following preparation steps:
[0070] The crushed stone, iron tailings sand, bauxite tailings powder and triisopropanolamine are mixed and stirred for 15 minutes, the crushed stone is iron tailings waste rock, the iron tailings waste rock is crushed, ground, and sieved to obtain a crushed stone with a particle size of 15 mm, the bauxite tailings powder is bauxite tailings coarse material calcined at 560°C for 40 minutes, the particle size of the bauxite tailings powder is 7μm, the iron tailings sand is firstly mixed with iron tailings coarse material and desulfurized gypsum and then ground for 50 minutes, the mass fraction of desulfurized gypsum in the iron tailings coarse material is 0.7wt%, and then the iron tailings sand is prepared by a sand making machine, and the fineness modulus of the iron tailings sand is 2.2-1.6. Then cement, water and modified straw fiber are added and stirred for 10 minutes to obtain concrete, the modified straw fiber is prepared by using Preparation Example 1, and the iron tailings sand cement uses P·O 42.5 ordinary Portland cement.
[0071] Example 2
[0072] A method for preparing low-carbon tailings concrete, which is different from Example 1 in that the iron tailings waste rock is crushed, ground, and sieved to obtain crushed stone with a particle size of 7 mm, the bauxite tailings powder is obtained by calcining the bauxite tailings coarse material at 450° C. for 30 minutes, and the particle size of the bauxite tailings powder is 6 μm, and the iron tailings sand is first obtained by mixing the iron tailings coarse material and desulfurization gypsum and then grinding it for 50 minutes, and the mass fraction of the desulfurization gypsum in the iron tailings coarse material is 0.5wt%.
[0073] Example 3
[0074] A method for preparing low-carbon tailings concrete, which is different from Example 1 in that the iron tailings waste rock is crushed, ground, and sieved to obtain crushed stone with a particle size of 20 mm, the bauxite tailings powder is obtained by calcining the bauxite tailings coarse material at 580°C for 45 minutes, and the particle size of the bauxite tailings powder is 10 μm. The iron tailings powder is first obtained by mixing the iron tailings coarse material and desulfurization gypsum and then grinding it for 50 minutes, and the mass fraction of the desulfurization gypsum in the iron tailings coarse material is 0.9wt%.
[0075] The components of the raw materials of Examples 1-3 and their corresponding weight parts are shown in Table 1.
[0076] Table 1 Raw materials and their weights in Examples 1-3 (kg)
[0077]
[0078]
[0079] Example 4
[0080] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 4.
[0081] Example 5
[0082] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 5.
[0083] Example 6
[0084] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 6.
[0085] Example 7
[0086] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 7.
[0087] Example 8
[0088] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 8.
[0089] Example 9
[0090] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 9.
[0091] Comparative Example
[0092] Comparative Example 1
[0093] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 10.
[0094] Comparative Example 2
[0095] A method for preparing low-carbon tailings concrete is different from Example 1 in that the modified straw fiber is prepared using Preparation Example 11.
[0096] Comparative Example 3
[0097] A method for preparing low-carbon tailings concrete, which is different from Example 1 in that the straw fiber is not modified, and the preparation of the concrete specifically includes the following preparation steps:
[0098] Crushed stone, iron tailings sand, bauxite tailings powder and triisopropanolamine were mixed and stirred for 15 minutes, and then cement, water and straw fiber were added and stirred for 10 minutes to obtain concrete.
[0099] Comparative Example 4
[0100] A method for preparing low-carbon tailings concrete is different from that of Example 1 in that the weight portion of the modified straw fiber is 15 kg, and the weights of the remaining components are the same as those of Example 1.
[0101] Comparative Example 5
[0102] A method for preparing low-carbon tailings concrete, which is different from Example 1 in that the weight portion of the modified straw fiber is 40 kg, and the weight of the remaining components is the same as that of Example 1.
[0103] Performance testing
[0104] Detection Methods
[0105] The concrete prepared in Examples 1-9 and Comparative Examples 1-4 was used as the test sample.
[0106] Slump and fluidity test standards: GB / T50080-2016 "Ordinary Concrete Mixture Performance Test Standard"; 28d compressive strength and 28d flexural strength test standards: GB / T50107-2010 "Concrete Strength Inspection and Evaluation Standard"; 28d limited shrinkage test standard: Tested in accordance with GB / T50082-2009 "Ordinary Concrete Long-term Performance and Durability Test Method Standard". Water penetration resistance: Test the water penetration depth of the standard test block in accordance with the step-by-step pressure method in GB / T50082-2009 "Ordinary Concrete Long-term Performance and Durability Test Method Standard".
[0107] Table 2 Performance test results
[0108]
[0109]
[0110] It can be seen from Example 1 and Examples 4-5 and Table 2 that by adjusting the appropriate concentration of the polyethylene glycol solution, a polyethylene glycol film is successfully coated on the surface of the straw fiber, solving the problem of decreased mechanical properties caused by the addition of a large amount of tailings.
[0111] Combining Example 1 with Examples 6-7 and Table 2, it can be seen that the various properties of Example 1 are better than those of Examples 6-7. The concentration of the polyethylene glycol solution affects the coating amount on the surface of the straw fiber. Therefore, the concentration of the polyethylene glycol should be controlled within a reasonable range. The coating film formed on the surface of the straw fiber dissolves and adheres to the surface of the tailings and cement colloid during the cement hydration process, thereby enhancing the interface bonding between the tailings and the cement colloid, improving the workability and fluidity of the concrete, and improving the mechanical properties of the concrete.
[0112] Combining Example 1 with Examples 8-9 and Table 2, it can be seen that the various properties of Example 1 are better than those of Examples 8-9. In the preparation process of the modified straw fiber, the amount of polyethylene glycol coated on the surface of the straw fiber is increased by soaking in an alkaline solution. Therefore, the performance is better than that of the sample that has not been soaked in the sodium hydroxide solution. Heating can intensify the movement of the polyethylene glycol molecular chain, which is more conducive to the coating of polyethylene glycol on the surface of the straw fiber.
[0113] When modified straw fiber is added to concrete, the polyethylene glycol on the surface of the straw fiber will soften and dissolve to a certain extent. In addition, the polyethylene glycol will adhere to the concrete matrix to form a coating film, reducing the contact between concrete and water and improving the concrete's later anti-seepage performance.
[0114] Combining Example 1 and Comparative Examples 1-4 with Table 2, it can be seen that high molecular weight polyethylene glycol is more conducive to polyethylene glycol coating due to the entanglement between molecular chains. When modified straw fibers are added to concrete, the mechanical properties and mixing properties of the concrete are better than those of the unmodified straw fibers.
[0115] Table 3 Anti-seepage performance test results
[0116] Example 1 Example 2 Example 3 Example 4 Example 5 Water penetration depth 4.3 4.4 4.5 4.6 4.5 Example 6 Example 7 Example 8 Example 9 Water penetration depth 5.0 5.3 6.2 6.0 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Water penetration depth 8.5 8.0 9.3 8.3 8.7
[0117] It can be seen from Table 3 that when modified straw fiber is added to concrete, the polyethylene glycol film on the surface of the straw fiber will adhere to the concrete matrix to form a coating film, reducing the contact between concrete and water and improving the later anti-permeability performance of concrete.
[0118] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A low-carbon tailings concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 70-80 parts of cement; 300-410 parts of crushed stone; Iron tailings 100-135 parts; Bauxite tailings powder 150-210 parts; 10-15 parts of triisopropanolamine; 20-35 parts of modified straw fiber; 35-55 parts water; The bauxite tailing powder is obtained by calcining bauxite tailing coarse materials at 450-580° C., and the modified straw fiber is obtained by modifying straw fiber through a step including polyethylene glycol coating, and the molecular weight of the polyethylene glycol is 6000-10000.
2. A low-carbon tailings concrete according to claim 1, characterized in that: The preparation method of the modified straw fiber comprises the following steps: crushing the straw fiber, soaking it in a sodium hydroxide solution, washing it with a hydrochloric acid solution until it becomes neutral after soaking, and drying it to obtain an initial dried product; then adding a polyethylene glycol solution to the initial dried product, heating it for reaction, and drying it to obtain the modified straw fiber.
3. A low-carbon tailings concrete according to claim 2, characterized in that: The mass concentration of the sodium hydroxide solution is 3-6wt%.
4. A low-carbon tailings concrete according to claim 2, characterized in that: The mass concentration of the polyethylene glycol solution is 7-11 wt %.
5. The low-carbon tailings concrete according to claim 1, characterized in that: The iron tailings sand has a silicon dioxide mass fraction of 27-30%, a aluminum oxide mass fraction of 8-11%, and a calcium oxide mass fraction of 20-25%.
6. The low-carbon tailings concrete according to claim 1, characterized in that: The mass fraction of aluminum oxide in the bauxite tailings powder is 40-45%, and the mass fraction of silicon dioxide is 30-37%.
7. The low-carbon tailings concrete according to claim 1, characterized in that: The calcination time of the bauxite tailings powder is 30-45 minutes.
8. The low-carbon tailings concrete according to claim 1, characterized in that: The iron tailings sand also includes an activation treatment step before use, and the activation treatment includes the following steps: mixing the iron tailings coarse material and desulfurization gypsum and then grinding them to obtain activated iron tailings powder, and then treating the activated iron tailings powder into iron tailings sand, wherein the mass fraction of the desulfurization gypsum in the iron tailings coarse material is 0.5-0.9wt%.
9. The method for preparing low-carbon tailings concrete according to any one of claims 1 to 8, characterized in that: The following steps are involved: The crushed stone, iron tailings sand, bauxite tailings powder and triisopropanolamine are mixed evenly, and then cement, water and the modified straw fiber are added and stirred evenly to obtain concrete.