An external electrode material used in 5GLTCC filter, 5GLTCC filter and preparation method thereof
By using external electrode materials containing ceramic powder in the LTCC filter, combined with spherical and flaky silver powder, glass powder, etc., the problem of poor matching of ceramics and silver paste is solved, and the mechanical properties and welding stability of the filter are improved. , improving the bending strength and thrust performance.
Patent Information
- Application Number
- CN202311308520.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-10-10
AI Technical Summary
The combination of ceramic materials and silver paste in existing LTCC filters lacks complete compatibility and special processing, resulting in stress concentration areas in the outer electrode after sintering, which affects the performance of the filter, especially poor performance in terms of bending strength and thrust. .
The external electrode material containing LTCC ceramic powder is used. The composition includes spherical silver powder, flake silver powder, glass powder, binder, thickener and ceramic powder. Through three-axis roller rolling and low-temperature sintering technology, the silver paste and ceramics are improved. The bonding force of the body slows down the shrinkage difference between the electrode and the ceramic body and enhances the welding stability.
It significantly improves the mechanical properties and welding stability of the filter, avoids dark cracking, improves the bending strength and ultimate thrust capabilities, and enhances the overall performance of the filter.
Smart Images

Figure CN117292869B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of filter electrode materials, and specifically relates to an external electrode material applied to a 5G LTCC filter, a 5G LTCC filter and a preparation method thereof. Background Art
[0002] Low Temperature Co-fired Ceramic (LTCC) technology has always been a popular process and technology in the active, passive and IC packaging industries, because LTCC uses low-loss dielectric ceramic materials and a multi-layer flexible design, which makes it easy to integrate the chip on the circuit board and has the best matching flexibility to adjust the circuit signal. Compared with the glass fiber substrate material used in traditional PCB materials, the reliability of LTCC process products is one level higher. Compared with other substrates such as HTCC and printed circuit boards, LTCC technology also has the advantages of material competitiveness and processing costs.
[0003] Multilayer LTCC devices can integrate antennas with front-end active devices such as RFIC or filters in an economical and efficient manner, which can further realize the process of circuit miniaturization and high density. These miniature LTCC RF modules are widely used in various communication devices such as smartphones, laptops, wearable devices, AR / VR applications, and are rapidly being applied in special fields such as aviation, communications, military, and medical care. Therefore, the materials and processes of LTCC filters have become the first choice for 5G high-frequency band components.
[0004] LTCC low-temperature co-fired ceramic technology is a technology that uses silver conductors to fill holes and print on cast green ceramic materials that have not been sintered at high temperatures to connect the internal circuit layers. The complex structure is laminated together through a multi-layer circuit design architecture, and then sintered at 850-900℃ to form an integrated multi-layer ceramic technology. In addition to providing the characteristics of the monomer itself, the ceramic material also relies on external electrodes to output the harmonic suppression capability within the monomer to achieve complete circuit integration, in order to complete the preparation of a complete LTCC filter element.
[0005] At present, the investment scale of domestic LTCC filter components in material research and development and product performance is still far behind that of overseas. The main reason is that overseas material manufacturers no longer simply develop ceramic powders, but can also develop suitable electrode pastes based on the characteristics of ceramic powders themselves and achieve mass production scale. Only by matching ceramic powders with silver paste can the performance of LTCC filter products be maximized.
[0006] At present, the combination of ceramic materials and silver paste for traditional LTCC filters is still in the stage of separate purchase and self-testing and adjustment, rather than complete matching, comprehensive, macroscopic analysis and special corresponding treatment. As a result, although the LTCC filter components currently produced can be used in terms of characteristics, they are still unable to reach certain key performance indicators. If this traditional method is continued, the product performance cannot be fundamentally improved. Moreover, since ceramics and external silver paste are two different substances with considerable differences, ceramics are oxides, and external silver paste is a metal substance. There is a great shrinkage mismatch between these two substances. Therefore, after silver sintering (Curing), the external electrode is prone to produce stress concentration areas at the corners of the product due to shrinkage mismatch forces. This stress concentration area is prone to dark cracks in the corners of the product after the bending strength test, affecting the performance of the filter. Summary of the invention
[0007] In view of the above-mentioned deficiencies in the prior art, the present invention provides an external electrode material applied to a 5G LTCC filter, a 5G LTCC filter and a preparation method thereof. The external electrode material has good compatibility with the LTCC material, can improve the mechanical properties and welding stability of the LTCC filter, further improve the performance of the filter, and solve the problems existing in the prior art.
[0008] To achieve the above purpose, the technical solution adopted by the present invention to solve the technical problem is:
[0009] An external electrode material used in a 5G LTCC filter, wherein the external electrode material contains ceramic powder having the same properties as that in the LTCC filter.
[0010] Furthermore, the invention comprises the following components in parts by weight: 70-80 parts of spherical silver powder, 4-6 parts of flaky silver powder, 3-5 parts of glass powder, 4-15 parts of binder, 1-5 parts of thickener, 0.5-5 parts of ceramic powder and 5-12 parts of solvent.
[0011] Furthermore, the particle size of the spherical silver powder is 1.2-3.0 μm, the particle size of the flaky silver powder is 2.5-5.0 μm, and the particle size of the glass powder is 0.5-2.5 μm.
[0012] Furthermore, the glass powder contains the following components in parts by weight: SiO 2 10-25 parts, BiO 3 20-40 parts, ZnO 2-5 parts, B 2 O 3 5-12 parts, MgO 2-6 parts.
[0013] Further, the binder includes at least one of ethyl cellulose, acrylic resin, polyvinyl alcohol and alkyd resin.
[0014] Further, the thickener includes at least one of methyl cellulose, hydroxyethyl cellulose, distearate, butylene glycol diacrylate and dipropylene phthalate.
[0015] Furthermore, the solvent is an organic acid, a ketone or an aromatic solvent.
[0016] Further, the solvent includes one of ethylene glycol ethyl ether acetate, ethyl acetate, xylene, methyl ethyl ketone, terpineol and diethylene glycol dimethyl ether.
[0017] Furthermore, the ceramic powder is BaO-WO 3 -SiO 2 -B 2 O 3 Co-synthesize oxides.
[0018] Furthermore, the ceramic powder contains the following components in parts by weight: 40-60 parts of BaO, 3 50-60 parts, SiO 2 2-5 parts and B 2 O 3 1-3 servings.
[0019] A 5G LTCC filter is made of the above-mentioned material, and the specific preparation method is as follows:
[0020] (1) mixing spherical silver powder, flake silver powder, glass powder, binder, thickener, ceramic powder and solvent at a speed of 250-500 rpm, and then transferring them into a three-axis roller for rolling and dispersion, and then filtering and degassing to obtain an external electrode paste;
[0021] (2) Cutting the LTCC product to obtain a green embryo monomer, and then placing the green embryo monomer in an external electrode paste so that the external electrode paste adheres to its surface; then, calcining the green embryo monomer adhered to the external electrode paste at 800-900° C. to obtain the product.
[0022] Furthermore, in step (1), the rotation speed of the three-axis roller is first set to 400-500 rpm, and the rolling is carried out for 5-7 minutes, and then the rotation speed of the three-axis roller is set to 250-300 rpm, and the rolling is carried out for 4-6 minutes.
[0023] The beneficial effects produced by the present invention are:
[0024] 1. In the present invention, spherical silver powder is used as the main material of the external electrode, which can increase the overall solid content and increase the electrode thickness. Flake silver powder is used as an auxiliary material. The large contact area of the flake silver powder increases the bonding degree between the external electrode and the LTCC ceramic body after sintering. However, it should not be added too much, otherwise burrs will easily appear.
[0025] Adding glass powder allows the external electrode material to form liquid phase sintering at low temperatures, while improving the density of silver powder at sintering temperatures below 900°C. Glass can also increase the adsorption effect on ceramics, allowing the glass to be adsorbed on the surface of the LTCC ceramic body at high temperatures, thereby greatly improving the bonding strength between the silver paste and the LTCC ceramic body. However, an appropriate amount should be added, otherwise it will increase the difficulty of subsequent electroplating processing or lead to insufficient bonding strength between the electrode and the ceramic body.
[0026] The binder is a high molecular polymer that can improve the coating and stability of the silver paste on the surface of the green embryo monomer. The binder is a thermoplastic and thermosetting material that can adhere to and solidify on the green embryo monomer the moment it contacts the green embryo monomer, and can be removed by sintering during subsequent high-temperature treatment without affecting the characteristics of the electrode.
[0027] Thickeners are polymer materials that can increase the viscosity of materials and make them form a stable gel for easy subsequent use;
[0028] The same ceramic powder as that in the LTCC ceramic body is added. The ceramic powder is the same as the ceramic in the green embryo monomer. During the high-temperature calcination process, the ceramic powder in the electrode gradually approaches the green embryo monomer and adheres to the green embryo monomer. This can slow down the shrinkage difference between the electrode and the ceramic green embryo monomer, reduce the problem of stress concentration around the product, and improve the product's ability to resist bending strength and ultimate thrust after welding.
[0029] 2. In the present invention, a three-axis roller is used to roll the silver powder particles at high speed to obtain a fine silver paste, and then low-speed rolling is performed to increase the residence time of the silver paste on the roller, so that the silver powder is rearranged and distributed in the paste, which can ensure that a silver paste with a high stacking density is obtained and the density of the silver paste after sintering is improved.
[0030] 3. The problem of weakened bending strength and increased thrust failure rate of the 5G LTCC components after boarding in the present invention can be solved by adding ceramic powder to the external electrode, which can completely avoid the problem of the components falling off the PCB circuit board after welding. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 are the thermal expansion curves of different materials;
[0032] Figure 2 This is a demonstration of dark cracks appearing after the traditional external electrode anti-bending test;
[0033] Figure 3 This is a physical picture of dark cracks appearing after the traditional external electrode anti-bending test;
[0034] Figure 4 This is a demonstration diagram of the external electrode of the present invention before silver firing;
[0035] Figure 5 This is a demonstration diagram of the external electrode of the present invention after silver sintering;
[0036] Figure 6 This is a physical picture of the dark cracks appearing on the outer electrode of the present invention after the bending resistance test;
[0037] Figure 7 Schematic diagram of a conventional outer electrode after being subjected to thrust rupture;
[0038] Figure 8 This is a physical picture of the traditional outer electrode after it was subjected to thrust fracture;
[0039] Fig. 9 It is a schematic diagram of the outer electrode of the present invention after being subjected to thrust rupture after application;
[0040] Fig.10 This is a real picture of the outer electrode of the present invention after being subjected to thrust rupture. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.
[0042] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0043] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0044] The features and performance of the present invention are further described in detail below in conjunction with the embodiments and drawings.
[0045] Example 1
[0046] An external electrode material for a 5G LTCC filter, the external electrode material containing ceramic powder having the same properties as that in the LTCC filter, specifically comprising the following components in parts by weight: 70 parts of spherical silver powder, 6 parts of flaky silver powder, 3 parts of glass powder, 10 parts of ethyl cellulose, 2 parts of methyl cellulose, 0.5 parts of ceramic powder and 8.5 parts of ethylene glycol ethyl ether acetate; wherein the particle size of the spherical silver powder is 1.2 μm, the particle size of the flaky silver powder is 2.5 μm, and the particle size of the glass powder is 0.5 μm; the glass powder contains the following components in parts by weight: SiO 2 10 parts, BiO 3 20 parts, ZnO 2 parts, B 2 O 3 5 parts, MgO 2 parts; the ceramic powder contains the following components by weight: BaO 40 parts, WO 3 50 parts, SiO 2 2 parts and B 2 O 3 1 serving;
[0047] A 5G LTCC filter is prepared using the above-mentioned material, and the specific preparation method is as follows:
[0048] (1) Spherical silver powder, flake silver powder, glass powder, binder, thickener, ceramic powder and solvent are stirred and mixed at a speed of 250-500 rpm, and then transferred into a three-axis roller, the speed of the three-axis roller is first set to 400 rpm, and the roller is rolled for 7 minutes, and then the speed of the three-axis roller is set to 250 rpm, and the roller is rolled for 6 minutes, and then filtered and degassed to obtain an external electrode paste;
[0049] (2) The LTCC product is cut to obtain a green embryo monomer, and then the green embryo monomer is placed in an external electrode paste so that the external electrode paste adheres to its surface; then, the green embryo monomer adhered to the external electrode paste is calcined at 800° C. to obtain the product.
[0050] Example 2
[0051] An external electrode material for a 5G LTCC filter, the external electrode material containing ceramic powder having homogeneity with that in the LTCC filter, specifically comprising the following components in parts by weight: 80 parts of spherical silver powder, 4 parts of flaky silver powder, 3 parts of glass powder, 4 parts of acrylic resin, 2 parts of hydroxyethyl fiber, 0.5 parts of ceramic powder and 6.5 parts of ethyl acetate; wherein the particle size of the spherical silver powder is 3.0 μm, the particle size of the flaky silver powder is 5.0 μm, and the particle size of the glass powder is 2.5 μm; the glass powder contains the following components in parts by weight: SiO 2 25 parts, BiO3 40 parts, ZnO 5 parts, B 2 O 3 12 parts, MgO 6 parts; the ceramic powder contains the following components by weight: BaO 60 parts, WO 3 60 parts, SiO 2 5 and B 2 O 3 3 servings;
[0052] A 5G LTCC filter is prepared using the above-mentioned material, and the specific preparation method is as follows:
[0053] (1) Spherical silver powder, flake silver powder, glass powder, binder, thickener, ceramic powder and solvent are stirred and mixed at a speed of 250-500 rpm, and then transferred into a three-axis roller, the speed of the three-axis roller is first set to 500 rpm, and the roller is rolled for 5 minutes, and then the speed of the three-axis roller is set to 300 rpm, and the roller is rolled for 4 minutes, and then filtered and degassed to obtain an external electrode paste;
[0054] (2) The LTCC product is cut to obtain a green embryo monomer, and then the green embryo monomer is placed in an external electrode paste so that the external electrode paste adheres to its surface; then, the green embryo monomer adhered to the external electrode paste is calcined at 900° C. to obtain the product.
[0055] Example 3
[0056] An external electrode material for a 5G LTCC filter, the external electrode material containing ceramic powder having homogeneity with that in the LTCC filter, specifically comprising the following components in parts by weight: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 0.5 parts of ceramic powder and 9.5 parts of xylene; wherein the particle size of the spherical silver powder is 2.0 μm, the particle size of the flaky silver powder is 3.5 μm, and the particle size of the glass powder is 1.5 μm; the glass powder contains the following components in parts by weight: SiO 2 20 parts, BiO 3 30 parts, ZnO 3 parts, B 2 O 3 8 parts, MgO 4 parts; the ceramic powder contains the following components by weight: BaO 50 parts, WO 3 55 parts, SiO 2 4 portions and B 2 O 3 2 servings;
[0057] A 5G LTCC filter is prepared using the above-mentioned material, and the specific preparation method is as follows:
[0058] (1) Spherical silver powder, flake silver powder, glass powder, binder, thickener, ceramic powder and solvent are stirred and mixed at a speed of 250-500 rpm, and then transferred into a three-axis roller, the speed of the three-axis roller is first set to 450 rpm, and the roller is rolled for 6 minutes, and then the speed of the three-axis roller is set to 300 rpm, and the roller is rolled for 5 minutes, and then filtered and degassed to obtain an external electrode paste;
[0059] (2) The LTCC product is cut to obtain a green embryo monomer, and then the green embryo monomer is placed in an external electrode paste so that the external electrode paste adheres to its surface; then, the green embryo monomer adhered to the external electrode paste is placed under 850° C. for calcination to obtain the product.
[0060] Example 4
[0061] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 1 part of ceramic powder and 9 parts of xylene, and the rest remain unchanged.
[0062] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0063] Example 5
[0064] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 1.5 parts of ceramic powder and 8.5 parts of xylene, and the rest remain unchanged.
[0065] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0066] Example 6
[0067] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 2 parts of ceramic powder and 8 parts of xylene, and the rest remain unchanged.
[0068] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0069] Example 7
[0070] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 2.5 parts of ceramic powder and 6.5 parts of xylene, and the rest remain unchanged.
[0071] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0072] Example 8
[0073] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 3 parts of ceramic powder and 7 parts of xylene, and the rest remain unchanged.
[0074] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0075] Example 9
[0076] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 3.5 parts of ceramic powder and 6.5 parts of xylene, and the rest remain unchanged.
[0077] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0078] Example 10
[0079] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 4 parts of ceramic powder and 6 parts of xylene, and the rest remain unchanged.
[0080] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0081] Embodiment 11
[0082] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 4.5 parts of ceramic powder and 5.5 parts of xylene, and the rest remain unchanged.
[0083] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0084] Example 12
[0085] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate, 5 parts of ceramic powder and 5 parts of xylene, and the rest remain unchanged.
[0086] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0087] Comparative Example 1
[0088] An external electrode material for a 5G LTCC filter. Based on Example 3, the specific components of the external electrode material are adjusted to: 73 parts of spherical silver powder, 4 parts of flaky silver powder, 5 parts of glass powder, 6 parts of polyvinyl alcohol, 2 parts of distearate and 10 parts of xylene, and the rest remain unchanged.
[0089] A LTCC filter applied to 5G, the preparation method is the same as that of Example 3.
[0090] The raw material parts used in Examples 1-12 and Comparative Example 1 are as follows:
[0091]
[0092]
[0093] Experimental example
[0094] 50 samples were prepared by the methods in Examples 1-12 and Comparative Example 1, and then the bending resistance and thrust performance of the samples prepared in Examples 1-12 and Comparative Example 1 were tested according to the automotive standard (AEC-Q200). The specific test results are shown in Tables 1 and Figure 1-8 .
[0095] Failure rate of bending strength = number of failed specimens / total number of specimens*100%
[0096] Thrust failure rate = number of failed samples / total number of samples*100%
[0097] Table 1: Performance results
[0098]
[0099] It can be seen from the above results that, compared with the filter element in Comparative Example 1, the bending failure rate and the reasoning failure rate of the filter element prepared by the method of the present invention are reduced, and the ultimate thrust is improved. The overall performance of the samples in Examples 1-12 is better than that of the sample in Comparative Example 1.
[0100] Figure 1 The thermal expansion curves of different materials show that there are certain differences in the thermal expansion properties of different materials.
[0101] Figure 2 This is a demonstration of dark cracks appearing after the traditional external electrode anti-bending test;
[0102] Figure 3 This is a real picture of dark cracks appearing after the traditional external electrode anti-bending test; it can be seen that dark cracks appear;
[0103] Figure 4 This is a demonstration diagram of the external electrode of the present invention before silver firing;
[0104] Figure 5 This is a demonstration diagram of the external electrode of the present invention after silver firing; it can be seen that the ceramic powder is concentrated near the ceramic green body;
[0105] Figure 6 This is a real picture of the dark cracks appearing on the outer electrode of the present invention after the bending resistance test; it can be seen that no dark cracks appear on the electrode;
[0106] Figure 7 Schematic diagram of a conventional outer electrode after being subjected to thrust rupture;
[0107] Figure 8 This is a physical picture of the traditional external electrode after it was subjected to thrust fracture. It can be seen that there is no silver on the surface of the product, which means that the ceramic body and the external electrode are not well bonded and the bonding force is poor;
[0108] Fig. 9 It is a schematic diagram of the outer electrode of the present invention after being subjected to thrust rupture after application;
[0109] Fig.10 This is a real picture of the outer electrode of the present invention after being subjected to thrust fracture. It can be seen that there is silver on the surface of the product, which means that the ceramic body and the outer electrode are well bonded and have stronger bonding force.
Claims
1. An external electrode material for 5G LTCC filter, characterized in that: The invention comprises the following components in parts by weight: 70-80 parts of spherical silver powder, 4-6 parts of flaky silver powder, 3-5 parts of glass powder, 4-15 parts of binder, 1-5 parts of thickener, 0.5-5 parts of ceramic powder having the same quality as that in LTCC filter, and 5-12 parts of solvent; The glass powder is composed of the following components in parts by weight: 10-25 parts of SiO2, 20-40 parts of Bi2O3, 2-5 parts of ZnO, 5-12 parts of B2O3, and 2-6 parts of MgO.
2. The external electrode material for 5G LTCC filter according to claim 1, characterized in that: The particle size of the spherical silver powder is 1.2-3.0 μm, the particle size of the flaky silver powder is 2.5-5.0 μm, and the particle size of the glass powder is 0.5-2.5 μm.
3. The external electrode material for 5G LTCC filter according to claim 1, characterized in that: The binder includes at least one of ethyl cellulose, acrylic resin, polyvinyl alcohol and alkyd resin.
4. The external electrode material for 5G LTCC filter according to claim 1, characterized in that: The thickener includes at least one of methyl cellulose, hydroxyethyl cellulose, distearate, butylene glycol diacrylate and dipropylene phthalate.
5. The external electrode material for 5G LTCC filter according to claim 1, characterized in that: The solvent is organic acid, ketone or aromatic.
6. The external electrode material for 5G LTCC filter according to claim 1, characterized in that: The ceramic powder is a BaO-WO3-SiO2-B2O3 co-synthesized oxide.
7. A LTCC filter for 5G, characterized in that: The material according to any one of claims 1 to 6 is used, and the specific preparation method is as follows: (1) mixing spherical silver powder, flake silver powder, glass powder, binder, thickener, ceramic powder and solvent at a speed of 250-500 rpm, and then transferring them into a three-axis roller for rolling, grinding and dispersion, and then filtering and degassing to obtain an external electrode paste; (2) Cutting the LTCC product to obtain a green embryo monomer, and then placing the green embryo monomer in an external electrode paste so that the external electrode paste adheres to its surface; then, calcining the green embryo monomer adhered to the external electrode paste at 800-900° C. to obtain the product.
Citation Information
Patent Citations
Conductive paste, lamination ceramics electronic assembly and method for manufacturing the electronic assembly
CN101154478A
Silver electrode slurry for environment-friendly dielectric ceramic filter and preparation method of silver electrode slurry
CN111128439A
Inner electrode paste and multilayer ceramic capacitor employing it
JP1996078267A
Conductive paste and layered ceramic capacitor
JP1997097518A
Ceramic electronic component and conductive paste therefor
JP2007294633A