A single crystal composite substrate and a method for preparing the same

By using pulsed laser radiation to process the amorphous phase deposition layer for recrystallization in the preparation of single crystal films and maintaining the substrate at room temperature, the problem of thermal mismatch stress during the high-temperature recrystallization process is solved, and a thicker and high-quality single crystal film is achieved. Preparation of crystalline composite substrates.

CN117568912BActive Publication Date: 2024-10-01SONGSHAN LAKE MATERIALS LAB +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311559095.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-21
Publication Date
2024-10-01
Estimated Expiration
2043-11-21

AI Technical Summary

Technical Problem

When preparing single crystal films of wide bandgap semiconductor materials, the internal stress caused by the thermal mismatch between the substrate and the film during the high-temperature recrystallization process leads to a decrease in material quality, making it difficult to prepare single crystal composite linings with thicker thickness and high quality. end.

Method used

The amorphous phase deposition layer is used for recrystallization through pulsed laser radiation treatment, keeping the substrate at room temperature, using structural defects as energy absorption centers to achieve high-quality recrystallization, and gradually increasing the thickness of the single crystal film through repeated deposition and recrystallization steps to avoid Stress introduced by thermal mismatch.

Benefits of technology

It effectively suppresses the thermal mismatch stress between the substrate and the single crystal film, improves the quality of the single crystal composite substrate, avoids the occurrence of cracks and structural defects, and realizes a thicker and high-quality single crystal composite substrate. preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117568912B_ABST
    Figure CN117568912B_ABST
Patent Text Reader

Abstract

The present application provides a single crystal composite substrate and a preparation method thereof, and relates to the field of composite materials. The preparation method of the single crystal composite substrate comprises the following steps: obtaining a single crystal composite substrate template, the single crystal composite substrate template comprising a substrate and a single crystal template formed on its surface; depositing a deposition layer on the surface of the single crystal template, the deposition layer being made of the same material as the single crystal template, and the deposition layer being an amorphous phase; treating the deposition layer with pulsed laser radiation to recrystallize the deposition layer, and obtaining a single crystal film, and keeping the substrate at room temperature during the recrystallization process; repeating the steps of deposition and recrystallization until the stacking thickness of the single crystal film reaches a preset thickness. The preparation method can reduce the internal stress between the substrate and the single crystal film on the basis of increasing the total thickness of the single crystal film, and effectively improve the quality of the single crystal composite substrate finally obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of composite materials, and in particular, to a single crystal composite substrate and a preparation method thereof. Background Art

[0002] With the advent of the era of big data and green energy, the development of new semiconductor materials and devices has become a bottleneck factor for the further development of society. The wide bandgap structure of wide bandgap semiconductor materials makes them inherently have more excellent material properties than the previous two generations of semiconductors, such as high temperature resistance, high pressure resistance, breakdown resistance, and radiation resistance.

[0003] Nevertheless, due to the extremely strong bond energy of the third generation, it is extremely difficult to prepare single crystal materials with high crystal quality, especially thin film materials with a certain thickness. The main difficulties come from two aspects. On the one hand, the recrystallization of the third generation semiconductors often requires extremely high temperatures, mostly above 1000 degrees Celsius, which itself brings extremely high challenges to the requirements of the preparation equipment; on the other hand, at this temperature, the thermal mismatch properties of the substrate material and the upper film area material will be highlighted, so that the upper single crystal film and the substrate area are subjected to huge internal stress, and this internal stress will cause cracks in the material and affect the yield on the one hand, and on the other hand, the stress will promote the generation of dislocations, thereby greatly reducing the quality of the single crystal material. Summary of the invention

[0004] The purpose of the embodiments of the present application is to provide a single crystal composite substrate and a method for preparing the same, which can produce a single crystal composite substrate with a total single crystal film thickness that is relatively thick, and during the preparation process can effectively suppress the stress introduced by thermal mismatch between the substrate and the single crystal film, thereby effectively improving the quality of the single crystal composite substrate finally obtained.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing a single crystal composite substrate, which comprises the following steps:

[0006] Obtaining a single crystal composite substrate template, the single crystal composite substrate template comprising a substrate and a single crystal template formed on a surface thereof;

[0007] Depositing a deposition layer on the surface of the single crystal template, the deposition layer is made of the same material as the single crystal template, and the deposition layer is an amorphous phase;

[0008] treating the deposited layer with pulsed laser radiation to recrystallize the deposited layer to obtain a single crystal film, wherein the substrate is kept at room temperature during the recrystallization process;

[0009] The steps of deposition and recrystallization are repeated until the stacking thickness of the single crystal film reaches a preset thickness.

[0010] In the above technical solution, a large number of structural defects in the amorphous phase deposition layer are utilized. The structural defects can serve as energy absorption centers in the subsequent pulsed laser radiation treatment to achieve a large amount of absorption of light radiation. At the same time, since the deposition layer is deposited on a single crystal template, it can induce high-quality recrystallization after a large amount of absorption of light radiation to obtain a high-quality single crystal film. And by keeping the substrate at room temperature during the recrystallization process, the internal stress introduced by the thermal mismatch between the substrate and the deposition layer during the recrystallization process is avoided, which is conducive to further improving the quality of the single crystal film. In summary, after repeated deposition and recrystallization steps, it is conducive to preparing a single crystal composite substrate with a thicker thickness and higher quality, avoiding the generation of cracks or structural defects.

[0011] In a possible implementation, the thickness of the deposited layer is less than or equal to 5 nm.

[0012] In one possible implementation, the power density of the pulsed laser radiation treatment is less than or equal to 1 J / cm 2 , the pulse time is within the millisecond order.

[0013] In a possible implementation manner, the deposition layer is formed by a physical vapor deposition method.

[0014] In a possible implementation, the growth temperature of the deposited layer is no greater than 600°C.

[0015] In a possible implementation, the pulse laser radiation treatment is performed in a protective atmosphere, where the protective atmosphere is used to suppress the decomposition of the surface of the deposited layer during the recrystallization process and to avoid the introduction of impurities.

[0016] In a possible implementation, the component of the deposited layer is nitride, and the protective atmosphere is nitrogen; or,

[0017] The composition of the deposited layer is oxide and the protective atmosphere is oxygen; or

[0018] The deposited layer is composed of silicon carbide and the protective atmosphere is methane.

[0019] In a possible implementation, the substrate includes silicon, sapphire, silicon carbide or gallium nitride, the single crystal template includes aluminum nitride, gallium nitride, silicon carbide or gallium oxide, and the material of the single crystal template is different from that of the substrate.

[0020] In a possible implementation, the light source used in the pulse laser radiation treatment is an ultrafast non-contact irradiation light source, and the ultrafast non-contact irradiation light source includes a xenon lamp, a flash lamp, or a pulse laser.

[0021] In a second aspect, an embodiment of the present application provides a single crystal composite substrate, which is manufactured by the above-mentioned manufacturing method. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is a schematic diagram of the preparation process of the single crystal composite substrate of the present application;

[0024] Figure 2 A schematic diagram of a single crystal film crystal surface of a single crystal composite substrate prepared in Example 1;

[0025] Figure 3 Schematic diagram of the single crystal film crystal surface of the single crystal composite substrate prepared in Comparative Example 1.

[0026] In the figure: 10 - single crystal composite substrate template; 11 - substrate; 12 - single crystal template; 20 - deposition layer; 30 - single crystal film. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0028] The single crystal composite substrate and the preparation method thereof according to the embodiment of the present application are described in detail below.

[0029] like Figure 1 As shown, the steps for preparing the single crystal composite substrate in the embodiment of the present application are specifically as follows:

[0030] S100 , obtaining a single crystal composite substrate template 10 , wherein the single crystal composite substrate template 10 comprises a substrate 11 and a single crystal template 12 formed on a surface thereof.

[0031] The materials of the substrate 11 and the single crystal template 12 are different. The substrate 11 includes but is not limited to silicon, sapphire, silicon carbide or gallium nitride. The orientation, size and doping conditions of the substrate 11 are not limited. The single crystal template 12 includes but is not limited to various single substances and compound semiconductor materials such as aluminum nitride, gallium nitride, silicon carbide or gallium oxide.

[0032] In some embodiments, the substrate 11 includes silicon, sapphire, silicon carbide or gallium nitride, the single crystal template 12 includes aluminum nitride, gallium nitride, silicon carbide or gallium oxide, and the material of the single crystal template 12 is different from that of the substrate 11. The single crystal template 12 is formed on the surface of the substrate 11 by, for example, MOCVD (Metal-Organic Chemical Vapor Deposition).

[0033] The single crystal template 12 is in a single crystal phase, and its surface is flat and crack-free, and its thickness is lower than the critical thickness of the material system of the single crystal template 12 for generating surface cracks.

[0034] S200, depositing a deposition layer 20 on the surface of the single crystal template 12, wherein the deposition layer 20 is made of the same material as the single crystal template 12, and the deposition layer 20 is in an amorphous phase.

[0035] The presence of a large number of structural defects in the amorphous phase deposition layer 20 is beneficial for the subsequent pulsed laser radiation treatment of the deposition layer 20 in step S300. The structural defects serve as energy absorption centers to absorb a large amount of light radiation. At the same time, since the deposition layer is deposited on the single crystal template 12, it can induce high-quality recrystallization after absorbing a large amount of light radiation, thereby obtaining a high-quality single crystal film 30.

[0036] Before the deposition layer 20 is deposited on the surface of the single crystal template 12, the single crystal composite substrate template 10 needs to be cleaned to avoid introducing impurities that affect the quality of the single crystal composite substrate finally obtained. The cleaning is generally performed by ultrasonically cleaning the single crystal composite substrate template 10 with acetone, ethanol, and deionized water in sequence, and then blowing the liquid on the surface with nitrogen.

[0037] In order to obtain the amorphous deposition layer 20 , in some embodiments, the deposition layer 20 is formed by physical vapor deposition.

[0038] Physical vapor deposition (PVD) is a process that evaporates (or sputters) metals, alloys or compounds in a vacuum chamber, so that these gas phase atoms or molecules are deposited on the surface of the workpiece under certain conditions. The preparation of amorphous phase can be achieved by controlling specific parameters. For details, please refer to related technologies.

[0039] Physical vapor deposition includes but is not limited to any thin film material growth method such as magnetron sputtering, reactive magnetron sputtering, molecular beam epitaxy, etc. Those skilled in the art can choose according to actual needs and are not limited here.

[0040] In some embodiments, the growth temperature of the deposition layer 20 is no greater than 600°C.

[0041] By limiting the growth temperature of the deposition layer 20 during the physical vapor deposition process, the introduction of thermal mismatch stress between the deposition layer 20 and the substrate 11 due to excessively high growth temperature can be alleviated or avoided, which is beneficial to improving the quality of the single crystal composite substrate.

[0042] S300 , treating the deposited layer 20 with pulsed laser radiation to recrystallize the deposited layer 20 , thereby obtaining a single crystal film 30 . During the recrystallization process, the substrate 11 is kept at room temperature.

[0043] It can be understood that the pulse laser radiation treatment is carried out at room temperature, and the temperature of the substrate 11 is kept at room temperature during the recrystallization process, which means that the substrate is originally at room temperature (the temperature of the substrate is room temperature, for example, 10-35°C), and during the pulse laser radiation treatment, the substrate 11 does not heat up and always maintains the same temperature as before the treatment. This can avoid the internal stress introduced by the thermal mismatch between the substrate 11 and the deposited layer 20 during the recrystallization process, which is beneficial to improving the quality of the single crystal film 30.

[0044] Figure 1 In the process of preparing the single crystal composite substrate, for the intermediate product, the interfaces between the multilayer single crystal films 30 and between the single crystal film 30 and the single crystal template 12 are represented by dotted lines.

[0045] Since there are a large number of structural defects in the deposition layer 20 prepared in step S200, when the deposition layer 20 is treated with pulsed laser radiation, the structural defects can serve as energy absorption centers to achieve a large amount of absorption of light radiation. At the same time, since the deposition layer 20 is deposited on the single crystal template 12, it can induce high-quality recrystallization after absorbing a large amount of light radiation to obtain a high-quality single crystal film 30.

[0046] Compared with continuous laser treatment, pulsed laser treatment can effectively avoid thermal mismatch caused by heat accumulation. In some embodiments, the light source used in pulsed laser radiation treatment is an ultra-fast non-contact irradiation light source, wherein the ultra-fast non-contact irradiation light source includes any one of non-contact irradiation light sources such as xenon lamp, flash lamp or pulsed laser, and those skilled in the art can select according to actual needs.

[0047] In some embodiments, the power density of the pulsed laser radiation treatment is less than or equal to 1 J / cm 2 , the pulse time is within the millisecond order.

[0048] That is, the present application adopts ultrafast light radiation to perform pulsed laser radiation processing, which is conducive to improving processing efficiency. The specific power density and pulse time can be selected for a specific composite substrate system, which can only achieve surface heating recrystallization but not enough to heat the substrate.

[0049] In some embodiments, the thickness of the deposition layer 20 is less than or equal to 5 nm.

[0050] On the one hand, the thin film 20 of the above thickness can be completely recrystallized to form a high-quality single crystal under the above pulse laser radiation processing parameters. On the other hand, due to its thin thickness, the pulse laser radiation treatment is actually an in-situ processing process, and the interface bonding strength between the formed single crystal films is high.

[0051] Since the surface of the deposited layer 20 decomposes when absorbing pulsed laser radiation energy for recrystallization, in some embodiments, the pulsed laser radiation treatment is performed in a protective atmosphere, which is used to inhibit the decomposition of the surface of the deposited layer 20 during the recrystallization process and not introduce impurities.

[0052] Exemplarily, the component of the deposition layer 20 is nitride, including but not limited to aluminum nitride, gallium nitride, etc., and the protective atmosphere is a nitrogen-rich atmosphere; or the component of the deposition layer 20 is oxide, including but not limited to nitride including but not limited to gallium oxide, etc., and the protective atmosphere is an oxygen-rich atmosphere, or the component of the deposition layer 20 is silicon carbide, etc., and the protective atmosphere is methane, etc.

[0053] The above arrangement is helpful to obtain a single crystal film 30 with a flat surface, thereby improving the quality of the single crystal composite substrate.

[0054] In some embodiments, the component of the deposited layer 20 is nitride, and the protective atmosphere is nitrogen; or, the component of the deposited layer 20 is oxide, and the protective atmosphere is oxygen; or, the component of the deposited layer 20 is silicon carbide, and the protective atmosphere is methane.

[0055] The protective atmosphere can effectively inhibit the surface of the deposited layer 20 from decomposing during the recrystallization process without introducing impurities.

[0056] S400 , repeating the steps of deposition and recrystallization until the stacking thickness of the single crystal film 30 reaches a preset thickness.

[0057] That is, a single crystal composite substrate having a relatively thick total thickness of the single crystal film 30 is finally obtained.

[0058] It should be noted that, since the single crystal film 30 and the single crystal template 12 prepared in each cycle in the single crystal composite substrate have the same composition and are both single crystals, the single crystal composite substrate finally prepared is actually composed of the substrate 11 and the thicker single crystal film. Figure 1 The dashed lines between the single crystal films 30 in the single crystal composite substrate finally obtained, and between the single crystal film 30 and the single crystal template 12 are shown in FIG.

[0059] Among them, the preset thickness can be selected according to actual needs, for example, the preset thickness is 1μm, 3μm, 5μm, 10μm, 30μm, etc. Technical personnel in this field can choose according to actual needs, and no limitation is made here.

[0060] The above preparation method can produce a single crystal composite substrate with a total single crystal film thickness that is relatively thick, and during the preparation process can effectively suppress the stress introduced by thermal mismatch between the substrate and the single crystal film, effectively improve the quality of the final single crystal composite substrate, and avoid the generation of cracks or structural defects.

[0061] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0062] Example 1

[0063] This embodiment provides a single crystal composite substrate, and the preparation method thereof is as follows:

[0064] (1) A single crystal composite substrate template was selected, and was cleaned by ultrasonic cleaning with ethanol and acetone for 10 minutes respectively, and then taken out and dried with nitrogen. The single crystal composite substrate template included a sapphire substrate and a single crystal aluminum nitride film with a thickness of 500 nm formed on the surface thereof.

[0065] (2) The single crystal composite substrate template is placed in a reactive magnetron sputtering device. The sputtering gas is a mixture of nitrogen and argon. The argon flow rate is 30 sccm, the nitrogen flow rate is 200 sccm, the chamber vacuum is 0.8 Pa, the sputtering power is 3000 W, and the sputtering temperature is 500°C. A single sputtering is performed to produce an amorphous aluminum nitride deposition layer with a thickness of 5 nm.

[0066] (3) Using visible light pulse laser to perform in-situ pulse irradiation annealing on the aluminum nitride deposition layer prepared by sputtering, the amorphous aluminum nitride deposition layer is recrystallized to form a single crystal aluminum nitride film. The laser used in the light irradiation treatment is a 532nm laser, and the laser spot area is 5×5mm 2 The background atmosphere is nitrogen atmosphere at normal pressure, the single pulse time is 30 nanoseconds, and the laser spot power density is 0.5 J / cm 2 It is expected that the temperature of the aluminum nitride deposition layer will instantly rise to over 2000°C, while the substrate will always remain at room temperature (around 25°C).

[0067] (4) One deposition process and one recrystallization process are repeated for 900 cycles, so that the total thickness of the final single-crystal aluminum nitride film increases to 5 μm, and finally the following is obtained: Figure 2 The sapphire-based aluminum nitride single crystal composite substrate shown is in a low stress state with no cracks on the surface.

[0068] Example 2

[0069] (1) A single crystal composite substrate template was selected, and ultrasonically cleaned with ethanol and acetone for 10 minutes respectively, and then taken out and dried with nitrogen. The single crystal composite substrate template included a silicon substrate and a single crystal aluminum nitride film with a thickness of 500 nm formed on the surface thereof.

[0070] (2) The single crystal composite substrate template is placed in a reactive magnetron sputtering device. The sputtering gas is a mixture of nitrogen and argon. The argon flow rate is 30 sccm, the nitrogen flow rate is 200 sccm, the chamber vacuum is 0.8 Pa, the sputtering power is 3000 W, and the sputtering temperature is 500°C. A single sputtering is performed to produce an amorphous aluminum nitride deposition layer with a thickness of 5 nm.

[0071] (3) Using visible light pulse laser to perform in-situ pulse irradiation annealing on the aluminum nitride deposition layer prepared by sputtering, the amorphous aluminum nitride deposition layer is recrystallized to form a single crystal aluminum nitride film. The laser used in the light irradiation treatment is a 532nm laser, and the laser spot area is 5×5mm 2 The background atmosphere is nitrogen atmosphere at normal pressure, the single pulse time is 30 nanoseconds, and the laser spot power density is 0.5 J / cm 2 It is expected that the temperature of the aluminum nitride deposition layer will instantly rise to over 2000°C, while the substrate will always remain at room temperature (around 25°C).

[0072] (4) One deposition process and one recrystallization process are repeated for 500 cycles, so that the total thickness of the final single-crystal aluminum nitride film is increased to 3 μm, and finally a silicon-based aluminum nitride single-crystal composite substrate in a low-stress state with no surface cracks is obtained.

[0073] Example 3

[0074] (1) A single crystal composite substrate template was selected, and ultrasonically cleaned with ethanol and acetone for 10 minutes respectively, and then taken out and dried with nitrogen. The single crystal composite substrate template included a silicon substrate and a single crystal gallium nitride film with a thickness of 500 nm formed on the surface of the silicon substrate.

[0075] (2) The single crystal composite substrate template was placed in a reactive magnetron sputtering device. The sputtering gas was a mixture of nitrogen and oxygen. The argon flow rate was 20 sccm, the oxygen flow rate was 200 sccm, and the chamber vacuum was 7×10 -1 Pa, the sputtering power is 3000 W, the sputtering temperature is 400° C., and an amorphous gallium nitride deposition layer with a thickness of 5 nm is obtained by single sputtering.

[0076] (3) Using a pulsed xenon lamp, the GaN deposited layer prepared by sputtering is subjected to in-situ pulsed irradiation annealing treatment to recrystallize the amorphous GaN deposited layer to form a single-crystal GaN film. The laser used in the light irradiation treatment is a 532nm laser, and the laser spot area is 5×5mm 2 The background atmosphere is oxygen at normal pressure, the single pulse time is 2 milliseconds, and the laser spot power density is 0.3 J / cm 2 .

[0077] (4) One deposition process and one recrystallization process are repeated for 590 cycles, so that the total thickness of the final single-crystal aluminum nitride film is increased to 3 μm, and finally a silicon-based gallium nitride single crystal composite substrate in a low-stress state with no surface cracks is obtained.

[0078] Comparative Example 1

[0079] This comparative example provides a single crystal composite substrate, and the preparation method thereof is different from that of Example 1 in that:

[0080] In step (2), the single crystal composite substrate template is placed in a reactive magnetron sputtering device, the sputtering gas is a mixture of nitrogen and argon, the argon flow rate is 30sccm, the nitrogen flow rate is 200sccm, the chamber vacuum is 0.8Pa, the sputtering power is 3000W, the sputtering temperature is 500°C, and the thickness of the aluminum nitride film prepared by sputtering is 2.5μm.

[0081] Then, the sapphire-based aluminum nitride single crystal composite substrate with a total thickness of 3 μm was obtained by heating and recrystallization at 1700 degrees Celsius. Figure 3 As shown, the surface of the obtained aluminum nitride film has hexagonal cracks with an angle of 60 degrees between the cracks, indicating that the stress formed by the substrate on the aluminum nitride film causes it to crack along the crystal direction, and the bonding force between the aluminum nitride film prepared by sputtering + high temperature annealing and the single crystal aluminum nitride film initially plated on the substrate is weak.

[0082] The above are only embodiments of the present application and are not intended to limit the scope of protection of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of protection of the present application.

Claims

1. A method for preparing a single crystal composite substrate, characterized in that: It includes the following steps: Obtaining a single crystal composite substrate template, wherein the single crystal composite substrate template comprises a substrate and a single crystal template formed on a surface thereof; Depositing a deposition layer on the surface of the single crystal template, wherein the deposition layer is made of the same material as the single crystal template and is an amorphous phase; Treating the deposited layer with pulsed laser radiation to recrystallize the deposited layer to obtain a single crystal film, wherein the substrate is kept at room temperature during the recrystallization process; Repeating the steps of deposition and recrystallization until the stacking thickness of the single crystal film reaches a preset thickness; the thickness of the deposited layer is less than or equal to 5 nm.

2. The method for preparing a single crystal composite substrate according to claim 1, characterized in that: The power density of the pulsed laser radiation treatment is less than or equal to 1J / cm 2 , the pulse time is within the millisecond order.

3. The method for preparing a single crystal composite substrate according to any one of claims 1 to 2, characterized in that: The deposition layer is formed by physical vapor deposition.

4. The method for preparing a single crystal composite substrate according to claim 3, characterized in that: The growth temperature of the deposited layer is no greater than 600°C.

5. The method for preparing a single crystal composite substrate according to any one of claims 1 to 2, characterized in that: The pulse laser radiation treatment is performed in a protective atmosphere, and the protective atmosphere is used to suppress the decomposition of the surface of the deposited layer during the recrystallization process and not introduce impurities.

6. The method for preparing a single crystal composite substrate according to claim 5, characterized in that: The component of the deposited layer is nitride, and the protective atmosphere is nitrogen; or, The component of the deposited layer is oxide, and the protective atmosphere is oxygen; or The component of the deposited layer is silicon carbide, and the protective atmosphere is methane.

7. The method for preparing a single crystal composite substrate according to any one of claims 1 to 2, characterized in that: The substrate includes silicon, sapphire, silicon carbide or gallium nitride, the single crystal template includes aluminum nitride, gallium nitride, silicon carbide or gallium oxide, and the material of the single crystal template is different from that of the substrate.

8. The method for preparing a single crystal composite substrate according to any one of claims 1 to 2, characterized in that: The light source used in the pulse laser radiation treatment is an ultra-fast non-contact irradiation light source, and the ultra-fast non-contact irradiation light source includes a xenon lamp, a flash lamp or a pulse laser.

9. A single crystal composite substrate, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of AlN film

    CN112795871A

  • High-quality aluminum nitride template and preparation method thereof

    CN113897678A

  • Aluminum nitride single-crystal composite substrate, preparation method thereof and ultraviolet light-emitting device

    CN115295401A

  • Recrystallization method of crystalline material

    CN115595670A

  • Method for making a monocristalline substrate and integrated circuit comprising such a substrate

    FR2819631A1