A repair membrane for preventing intrauterine adhesions and its preparation method and application

The repair membrane with a double-layer structure prepared by electrospinning technology solves the problems of poor biocompatibility and difficult to control degradation time in the existing technology, achieves effective prevention and treatment of intrauterine adhesions, and promotes tissue repair and regeneration.

CN117582560BActive Publication Date: 2024-10-15SHENZHEN ZHIPEPTIDE AESTHETIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311296502.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-09
Publication Date
2024-10-15
Estimated Expiration
2043-10-09

AI Technical Summary

Technical Problem

In terms of preventing and treating intrauterine adhesions, existing repair membranes have problems such as poor biocompatibility, difficult to control degradation time and side effects of metabolites, and cannot effectively prevent intrauterine adhesions.

Method used

A repair membrane with a double-layer structure is prepared using electrospinning technology. The inner layer has an anti-inflammatory effect and the outer layer promotes local repair. By adding sericin, polyethylene glycol (PEG) and glycyrrhizic acid to the silk fibroin solution Based on DES, as well as short peptides, a composite repair film is formed, which is combined with steam fumigation and ethanol soaking treatments to improve flexibility.

Benefits of technology

It achieves good biocompatibility and biodegradability of the repair membrane in the body, effectively prevents uterine cavity adhesion, promotes tissue repair and regeneration, and exerts a physical anti-adhesion effect and slowly releases short peptides through a double-layer structure to promote uterine cavity repair. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117582560B_ABST
    Figure CN117582560B_ABST
Patent Text Reader

Abstract

The invention discloses a repair film for preventing intrauterine adhesion, and a preparation method and application thereof, which belong to the field of medicine. The invention first prepares an inner layer solution and an outer layer solution respectively, and then spins the inner layer solution by electrostatic spinning technology, and then spins the outer layer solution on the basis of the inner layer to obtain the repair film. The repair film of the invention has a double-layer structure, and the inner layer repair film has an anti-inflammatory effect, which can effectively prevent the occurrence of intrauterine adhesion; the outer layer repair film has the function of promoting local repair, which can effectively promote the repair and regeneration of tissues, and can more effectively and safely prevent and treat intrauterine adhesion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a repair membrane, in particular to a repair membrane for preventing intrauterine adhesion prepared by electrostatic spinning technology and application thereof. Background Art

[0002] Intrauterine adhesion is a common complication that often occurs after endometrial ablation, abortion, myomectomy and other surgeries. Intrauterine adhesion can cause irregular menstruation, infertility and other problems, causing great pain to patients. At present, the methods for preventing and treating intrauterine adhesion are not ideal, and more effective and safe methods are needed to prevent and treat intrauterine adhesion.

[0003] Existing repair membranes are mostly made of polymer materials, such as PLGA, PVA, etc., which often have problems such as poor biocompatibility, difficult to control degradation time, and side effects of metabolites. Summary of the invention

[0004] In order to achieve the above-mentioned purpose, the present invention provides a repair membrane for preventing intrauterine adhesion and a preparation method thereof. The repair membrane of the present invention has a double-layer structure. The inner repair membrane has an anti-inflammatory effect and can effectively prevent the occurrence of intrauterine adhesion; the outer repair membrane has the function of promoting local repair, which can effectively promote the repair and regeneration of tissues, and can more effectively and safely prevent and treat intrauterine adhesion.

[0005] First, the present invention provides a method for preparing a repair membrane for preventing intrauterine adhesions, the preparation method comprising the following steps: firstly, preparing an inner layer solution and an outer layer solution respectively, then spinning the inner layer solution by using an electrospinning technique, and then spinning the outer layer solution on the basis of the inner layer to obtain the repair membrane;

[0006] The inner layer solution is prepared by adding sericin, polyethylene glycol (PEG) and glycyrrhizic acid-based DES to a 10-30wt% silk fibroin solution, so that the sericin content is 0.1-2wt%, the polyethylene glycol (PEG) content is 0.1-2wt%, the glycyrrhizic acid-based DES content is 0.1-5wt%, and the solvent is water;

[0007] The outer layer solution is prepared by adding PEG and short peptides to a 10-30wt% silk fibroin solution, so that the content of PEG is 0.1-2wt%, the content of short peptide is 0.1-5wt%, and the solvent is water.

[0008] In one embodiment of the present invention, the molecular weight of the polyethylene glycol is 10,000-100,000.

[0009] In one embodiment of the present invention, any one or more of arginine, betaine, and proline and glycyrrhizic acid are weighed at a molar ratio of 1:1-1:5, respectively, and heated and stirred at 40-50° C. for 6-24 hours to obtain glycyrrhizic acid-based DES.

[0010] In one embodiment of the present invention, the sequence of the short peptide is one or more of KIIK (SEQ NO ID: 1), KKIIKK (SEQ NO ID: 2), RRIIRR (SEQ NO ID: 3), KRIIIIKR (SEQ NOID: 4), RRIIIIRR (SEQ NO ID: 5) or KKIIIIKK (SEQ NO ID: 6).

[0011] In one embodiment of the present invention, the volume ratio of the solution of the inner layer to that of the outer layer is 1-3:1-3.

[0012] In one embodiment of the present invention, the parameters of the electrospinning are: voltage: 10-30 kV; current: 0.1-1 mA; nozzle distance: 10-20 cm; rotation speed: 500-2000 rpm.

[0013] In one embodiment of the present invention, the preparation method of the present invention specifically comprises the following steps:

[0014] Preparation of inner layer solution:

[0015] Step 1: preparing a silk fibroin solution, and reverse dialysing the silk fibroin solution in PEG6000-50000 to obtain a silk fibroin concentrated solution with a concentration of 10-30%;

[0016] Step 2: Add sericin to the above fibroin concentrated solution to make the concentration of sericin 0.1-2%;

[0017] Step 3: Add PEG10000-100000 to the mixed solution in step 2 to make the concentration of PEG10000-100000 be 0.1-2%;

[0018] Step 4: Add glycyrrhizic acid DES to the mixed solution in step 3 to make the concentration of glycyrrhizic acid DES 0.1%-5%;

[0019] Preparation of outer layer solution:

[0020] Step 5: preparing a silk fibroin solution, and reverse dialysing the silk fibroin solution in PEG 6000-50000 to obtain a concentrated silk fibroin solution with a concentration of 10-30%;

[0021] Step 6: dissolving the short peptide and PEG10000-100000 in the silk fibroin concentrate, wherein the short peptide and PEG10000-100000 account for 0.1%-5% and 0.1-2% of the total mass, respectively;

[0022] Step 7: Prepare a repair membrane through electrospinning technology, first spin the inner layer solution, and then spin the outer layer solution based on the electrospinning of the inner layer solution to obtain a composite repair membrane.

[0023] In one embodiment of the present invention, the obtained composite repair film is fumigated with water vapor.

[0024] In one embodiment of the present invention, a treatment process of soaking in 70-75% ethanol for 1-8 hours can be added after steam fumigation to improve the flexibility of the repair film.

[0025] Secondly, the present invention also provides a repair membrane for preventing intrauterine adhesions prepared by the above preparation method.

[0026] In one embodiment of the present invention, the inner repair membrane has an anti-inflammatory effect and can effectively prevent the occurrence of intrauterine adhesions; the outer repair membrane has the function of promoting local repair and can effectively promote tissue repair and regeneration.

[0027] Finally, the present invention also provides a medical device, which comprises the above-mentioned repair membrane.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] (1) The repair membrane has good biocompatibility and biodegradability when used in vivo and can effectively promote tissue repair and regeneration.

[0030] (2) This repair membrane has a double-layer structure, which can not only exert a physical anti-adhesion effect, but also slowly release short peptides and DES to promote uterine cavity repair.

[0031] (3) Compared with freeze-dried films or films formed by natural air drying, the thickness of the repair film of the present invention can be more finely controlled. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Actual picture of the electrospinning membrane prepared in Example 1.

[0033] Figure 2 Microscopic morphology of the electrospun membrane prepared in Example 1.

[0034] Figure 3 Mechanical properties of the electrospun membrane prepared in Example 1.

[0035] Figure 4Cell viability graph of the electrospun membrane prepared in Example 1. DETAILED DESCRIPTION

[0036] The present invention is further explained in detail below through specific examples, but they are not intended to limit the present invention and are merely illustrative.

[0037] Silk fibroin and sericin are extracted by ourselves.

[0038] Embodiment 1:

[0039] Preparation of DES

[0040] Arginine and glycyrrhizic acid powders were weighed into a sample bottle at a molar ratio of 1:2, heated (40° C.) and stirred for 12 hours to obtain arginine glycyrrhizic acid DES.

[0041] Preparation of inner layer solution

[0042] Silk fibroin was extracted from cooked silk (refer to Example 1 of CN 107412872 B, the same below), and concentrated with PEG10000 to obtain a 20% silk fibroin solution; sericin was added to the silk fibroin concentrate (the preparation method of sericin is referred to CN 114874304 B, the same below) to make the sericin account for 0.1% of the total mass; PEG10000 was added to the above mixed solution to make PEG account for 0.1% of the total mass; arginine glycyrrhizic acid DES was added to the above solution to make the content of DES account for 0.1% of the total mass; the above solutions were mixed evenly and allowed to stand at room temperature for stabilization.

[0043] Preparation of outer layer solution

[0044] Silk fibroin is extracted from cooked silk, and PEG10000 is used to concentrate the silk fibroin to obtain a 20% silk fibroin solution; PEG10000 is added to the silk fibroin concentrate to make PEG account for 0.1% of the total mass; a short peptide is added to the above solution to make the content of the short peptide account for 0.5% of the total mass (the short peptide is KKIIIIKK); the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0045] Preparation of repair membranes by electrospinning

[0046] The inner and outer repair membranes were prepared successively by electrospinning technology, and the electrospinning parameters were: voltage: 20 kV; current: 0.1 mA; nozzle distance: 12 cm; rotation speed: 600 rpm.

[0047] The volume ratio of the inner layer to the outer layer solution is 1:1.

[0048] Post-processing

[0049] Finally, the electrospun membrane was fumigated with water vapor for 24 h.

[0050] Embodiment 2:

[0051] Preparation of DES

[0052] Proline and glycyrrhizic acid powders were weighed into a sample bottle at a molar ratio of 1:3, and heated (50° C.) and stirred for 16 hours to obtain proline glycyrrhizic acid DES.

[0053] Preparation of inner layer solution

[0054] Silk fibroin is extracted from cooked silk, and PEG20000 is used to concentrate the silk fibroin to obtain a 18% silk fibroin solution; sericin is added to the silk fibroin concentrate to make the sericin account for 0.2% of the total mass; PEG20000 is added to the above mixed solution to make the PEG account for 0.2% of the total mass; proline glycyrrhizic acid DES is added to the above solution to make the DES content account for 0.5% of the total mass; the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0055] Preparation of outer layer solution

[0056] Silk fibroin is extracted from cooked silk, and PEG10000 is used to concentrate the silk fibroin to obtain a 20% silk fibroin solution; PEG20000 is added to the silk fibroin concentrate to make PEG account for 0.3% of the total mass; a short peptide is added to the above solution to make the content of the short peptide account for 0.5% of the total mass (the short peptide is RRIIIIRR); the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0057] Preparation of repair membranes by electrospinning

[0058] The inner and outer repair membranes were prepared by electrospinning technology. The electrospinning parameters were: voltage: 22 kV; current: 0.2 mA; nozzle distance: 16 cm; rotation speed: 800 rpm

[0059] The volume ratio of the inner layer to the outer layer solution is 1:1.

[0060] Post-processing

[0061] Finally, the electrospun membrane was fumigated with water vapor for 48 h.

[0062] Embodiment 3:

[0063] Preparation of DES

[0064] Betaine and glycyrrhizic acid powders were weighed into a sample bottle at a molar ratio of 1:3, heated (50° C.) and stirred for 16 hours to obtain betaine glycyrrhizic acid DES.

[0065] Preparation of inner layer solution

[0066] Silk fibroin is extracted from cooked silk, and PEG30000 is used to concentrate the silk fibroin to obtain a 25% silk fibroin solution; sericin is added to the silk fibroin concentrate to make the sericin account for 0.4% of the total mass; PEG50000 is added to the above mixed solution to make the PEG account for 0.2% of the total mass; betaine glycyrrhizic acid DES is added to the above solution to make the DES content account for 1% of the total mass; the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0067] Preparation of outer layer solution

[0068] Silk fibroin is extracted from cooked silk, and PEG30000 is used to concentrate the silk fibroin to obtain a 25% silk fibroin solution; PEG50000 is added to the silk fibroin concentrate to make PEG account for 0.2% of the total mass; a short peptide is added to the above solution to make the content of the short peptide account for 1% of the total mass (the short peptide is KIIK); the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0069] Preparation of repair membranes by electrospinning

[0070] The inner and outer repair membranes were prepared by electrospinning technology. The electrospinning parameters were: voltage: 23 kV; current: 0.1 mA; nozzle distance: 15 cm; rotation speed: 400 rpm

[0071] The volume ratio of the inner layer to the outer layer solution is 1:1.

[0072] Post-processing

[0073] Finally, the electrospun membrane was fumigated with water vapor for 24 h.

[0074] Embodiment 4:

[0075] Preparation of DES

[0076] Arginine and glycyrrhizic acid powders were weighed into a sample bottle at a molar ratio of 1:2, heated (40° C.) and stirred for 12 hours to obtain arginine glycyrrhizic acid DES.

[0077] Preparation of inner layer solution

[0078] Silk fibroin is extracted from cooked silk, and concentrated using PEG20000 to obtain a silk fibroin solution with a concentration of 18%; sericin is added to the silk fibroin concentrate so that the sericin accounts for 0.1% of the total mass; PEG30000 is added to the above mixed solution so that the PEG accounts for 0.1% of the total mass; arginine glycyrrhizic acid DES is added to the above solution so that the content of DES accounts for 0.1% of the total mass; the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0079] Preparation of outer layer solution

[0080] Silk fibroin is extracted from cooked silk, and PEG20000 is used to concentrate the silk fibroin to obtain a 18% silk fibroin solution; PEG30000 is added to the silk fibroin concentrate to make PEG account for 0.1% of the total mass; a short peptide is added to the above solution to make the content of the short peptide account for 0.5% of the total mass (the short peptide is KKIIIIKK); the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0081] Preparation of repair membranes by electrospinning

[0082] The inner and outer repair membranes were prepared successively by electrospinning technology, and the electrospinning parameters were: voltage: 18 kV; current: 0.1 mA; nozzle distance: 12 cm; rotation speed: 600 rpm.

[0083] The volume ratio of the inner layer to the outer layer solution is 2:1.

[0084] Post-processing

[0085] Finally, the electrospun membrane was fumigated with water vapor for 24 h.

[0086] Embodiment 5:

[0087] Preparation of DES

[0088] Proline and glycyrrhizic acid powders were weighed into a sample bottle at a molar ratio of 1:2, heated (40° C.) and stirred for 12 hours to obtain proline glycyrrhizic acid DES.

[0089] Preparation of inner layer solution

[0090] Silk fibroin is extracted from cooked silk, and PEG30000 is used to concentrate it to obtain a silk fibroin solution with a concentration of 15%; sericin is added to the silk fibroin concentrate so that the sericin accounts for 1.5% of the total mass; PEG40000 is added to the above mixed solution so that PEG accounts for 1.0% of the total mass; proline glycyrrhizic acid DES is added to the above solution so that the content of DES accounts for 2.1% of the total mass; the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0091] Preparation of outer layer solution

[0092] Silk fibroin is extracted from cooked silk, and PEG30000 is used to concentrate the silk fibroin to obtain a 20% silk fibroin solution; PEG40000 is added to the silk fibroin concentrate to make PEG account for 0.1% of the total mass; a short peptide is added to the above solution to make the content of the short peptide account for 3.0% of the total mass (the short peptide is RRIIRR); the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0093] Preparation of repair membranes by electrospinning

[0094] The inner and outer repair membranes were prepared successively by electrospinning technology, and the electrospinning parameters were: voltage: 20 kV; current: 0.1 mA; nozzle distance: 12 cm; rotation speed: 600 rpm.

[0095] The volume ratio of the inner layer to the outer layer solution is 1:2.

[0096] Post-processing

[0097] Finally, the electrospun membrane was fumigated with water vapor for 48 h.

[0098] Embodiment 6:

[0099] Preparation of DES

[0100] Arginine and glycyrrhizic acid powders were weighed into a sample bottle at a molar ratio of 1:4, and heated (40° C.) and stirred for 12 hours to obtain arginine glycyrrhizic acid DES.

[0101] Preparation of inner layer solution

[0102] Silk fibroin is extracted from cooked silk, and concentrated with PEG50000 to obtain a 25% silk fibroin solution; sericin is added to the silk fibroin concentrate so that the sericin accounts for 0.1% of the total mass; PEG80000 is added to the above mixed solution so that the PEG accounts for 0.1% of the total mass; arginine glycyrrhizic acid DES is added to the above solution so that the content of DES accounts for 0.1% of the total mass; the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0103] Preparation of outer layer solution

[0104] Silk fibroin is extracted from cooked silk, and PEG50000 is used to concentrate the silk fibroin to obtain a 25% silk fibroin solution; PEG80000 is added to the silk fibroin concentrate to make PEG account for 0.1% of the total mass; a short peptide is added to the above solution to make the content of the short peptide account for 0.5% of the total mass (the short peptide is KKIIIIKK); the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0105] Preparation of repair membranes by electrospinning

[0106] The inner and outer repair membranes were prepared successively by electrospinning technology, and the electrospinning parameters were: voltage: 25 kV; current: 0.1 mA; nozzle distance: 12 cm; rotation speed: 600 rpm.

[0107] The volume ratio of the inner layer to the outer layer solution is 1:3.

[0108] Post-processing

[0109] Finally, the electrospun membrane was fumigated with water vapor for 24 h.

[0110] Example 7: Application

[0111] L929 cells were used to model cell scratches, and then the scratch model cells were treated with the repair membrane extract (refer to the national standard GB / T16886), and the scratch area was calculated at 0 hours, 24 hours, and 48 hours, and the repair rate was calculated using imageJ software. It can be seen that the repair membrane prepared by the present invention has a more obvious repair effect on cell scratches. Similarly, the repair membrane prepared in Examples 4 to 6 was tested according to the above method, and its repair rate after 72 hours can reach more than 50%.

[0112] Table 1 Repair effect of the repair membranes prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2 on intrauterine adhesions

[0113]

[0114] The repaired film was stretched by a universal tensile machine to test the stretching effect of the film. Figure 3 As shown, the membrane was stretched to three times its own length without breaking, proving that it has good tensile properties and meets the requirements for use of uterine cavity repair membranes.

[0115] L929 cells were treated with 0%, 25%, 75% and 100% of the repair membrane extract, respectively, which proved that the repair membrane extract had no damage to the cells (refer to the national standard GB / T16886).

[0116] Example 8: Optimization

[0117] The physical properties and biological activity of the repair membrane can be improved by optimizing the composition ratio of the inner and outer repair membranes, the electrospinning process parameters, etc., thereby further improving the therapeutic effect and safety of the repair membrane.

[0118] Table 2 Effect of electrospinning process parameters on water absorption

[0119]

[0120] After steam fumigation, 70-75% ethanol can be added for soaking for 0.5-8h to improve the water absorption rate of the repair film.

[0121] Table 3 Changes in water absorption of repaired membranes after ethanol immersion

[0122]

[0123] Comparative Example 1

[0124] Silk fibroin is extracted from cooked silk, and PEG10000 is used to concentrate the silk fibroin to prepare a 20% silk fibroin solution; sericin is added to the silk fibroin concentrate to make the sericin account for 0.1% of the total mass; PEG10000 is added to the aforementioned mixed solution to make the PEG10000 account for 0.1% of the total mass; the aforementioned solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0125] The repair membrane was prepared by electrospinning technology, and the electrospinning parameters were: voltage: 20 kV; current: 0.1 mA; nozzle distance: 12 cm; rotation speed: 600 rpm.

[0126] Comparative Example 2

[0127] Silk fibroin is extracted from cooked silk, and PEG10000 is used to concentrate the silk fibroin to obtain a 20% silk fibroin solution; PEG10000 is added to the silk fibroin concentrate to make PEG10000 account for 0.1% of the total mass; a short peptide is added to the above solution to make the content of the short peptide account for 0.5% of the total mass (the short peptide is KKIIIIKK); the above solutions are mixed evenly and allowed to stand at room temperature to stabilize.

[0128] Preparation of repair membranes by electrospinning

[0129] The inner and outer repair membranes were prepared successively by electrospinning technology, and the electrospinning parameters were: voltage: 20 kV; current: 0.1 mA; nozzle distance: 12 cm; rotation speed: 600 rpm.

[0130] In summary, the present invention provides a repair membrane for preventing intrauterine adhesions prepared by electrospinning technology, which has good biocompatibility and biodegradability, can effectively prevent the occurrence of intrauterine adhesions, promote tissue repair and regeneration, and has broad application prospects.

[0131] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a repair membrane for preventing intrauterine adhesions, It is characterized in that The preparation method comprises the following steps: firstly, preparing an inner layer solution and an outer layer solution respectively, then spinning the inner layer solution by using electrostatic spinning technology, and then spinning the outer layer solution on the basis of the inner layer to obtain the repair membrane; The inner layer solution is prepared by adding sericin, polyethylene glycol and glycyrrhizic acid-based DES to a 10-30 wt% silk fibroin solution, so that the sericin content is 0.1-2 wt%, the polyethylene glycol content is 0.1-2 wt%, and the glycyrrhizic acid-based DES content is 0.1-5 wt%; The outer layer solution is prepared by adding polyethylene glycol and short peptides to a 10-30 wt% silk fibroin solution, so that the content of polyethylene glycol is 0.1-2 wt% and the content of short peptides is 0.1-5 wt%; The sequence of the short peptide is one or more of KIIK, KKIIKK, RRIIRR, KRIIIIKR, RRIIIIRR or KKIIIIKK; The glycyrrhizic acid-based DES is prepared by the following method: any one or more of arginine, betaine, and proline and glycyrrhizic acid are weighed respectively according to a molar ratio of 1:1-1:5, and heated and stirred at 40-50° C. for 6-24 hours to obtain the glycyrrhizic acid-based DES.

2. A method for preparing a repair membrane for preventing intrauterine adhesion according to claim 1, It is characterized in that The molecular weight of the polyethylene glycol is 10,000-100,000.

3. A method for preparing a repair membrane for preventing intrauterine adhesion according to claim 1, It is characterized in that The volume ratio of the inner layer and the outer layer solution is 1~3:1~3.

4. A method for preparing a repair membrane for preventing intrauterine adhesion according to claim 1, It is characterized in that The parameters of the electrospinning are: voltage: 10-30 kV; current: 0.1-1 mA; nozzle distance: 10-20 cm; rotation speed: 500-2000 rpm.

5. A method for preparing a repair membrane for preventing intrauterine adhesion according to any one of claims 1 to 4, It is characterized in that The obtained composite repair film is fumigated with water vapor.

6. A method for preparing a repair membrane for preventing intrauterine adhesion according to claim 5, It is characterized in that After steam fumigation, add 70-75% ethanol soaking for 1-8 hours.

7. A repair membrane for preventing intrauterine adhesions prepared according to the method for preparing a repair membrane for preventing intrauterine adhesions according to any one of claims 1 to 6.

8. A medical device, It is characterized in that The medical device comprises the repair membrane according to claim 7.