Solar cell and metallization method thereof

By using nanomaterials with a core-shell structure to form a mesh electrode pattern, the problems of large shading area, high resistance and large amount of silver paste used in solar cell metallization technology are solved, and the resistance, shading area and silver consumption are reduced. , reducing battery manufacturing costs.

CN117637902BActive Publication Date: 2024-10-29TRINA SOLAR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311448149.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-01
Publication Date
2024-10-29
Estimated Expiration
2043-11-01

AI Technical Summary

Technical Problem

Existing solar cell metallization technology has problems such as large shading area, high resistance, large amount of silver paste used, and high cost of raw materials and equipment.

Method used

Nanomaterials with a core-shell structure are used instead of silver paste, a liquid film is formed through a solution method, and the metal nanoparticles are connected to the doping layer through sintering to form an electrode pattern with a network structure, and spaced connecting lines are prepared to collect current and reduce Resistance and shading area, reducing the amount of silver.

Benefits of technology

It has achieved reduced resistance, reduced light-shielding area, and reduced silver consumption by more than 30%, reducing the manufacturing cost of crystalline silicon cells, and the process is simple and the cost is low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117637902B_ABST
    Figure CN117637902B_ABST
Patent Text Reader

Abstract

The present application relates to the field of optoelectronic technology, and in particular to a solar cell and a method for preparing the same. The purpose is to solve the problems of large shading area, large resistance, and large amount of silver paste used in the battery metallization technology in the related art. A method for metallizing a solar cell, comprising: providing a silicon substrate, a doping layer formed on the surface of the silicon substrate; preparing a solution of a nanomaterial with a core-shell structure, wherein the core of the core-shell structure is a metal nanoparticle, and the shell at least comprises: an inorganic nanomaterial contained in glass powder; applying the solution of the nanomaterial with a core-shell structure to the surface of the doping layer away from the silicon substrate to form a liquid film; sintering the liquid film so that the metal nanoparticles are connected into a mesh structure, and connected to the silicon in the doping layer to form a silicon alloy; forming a connecting line on the surface of the mesh structure away from the silicon substrate, and the connecting line is used to collect the current flowing through the mesh structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of optoelectronic technology, and in particular to a solar cell and a metallization method thereof. Background Art

[0002] With the development of solar cell technology, it is particularly important to reduce production costs while continuously improving the photoelectric conversion efficiency of solar cells.

[0003] Thinning the front grid lines is an effective solution to improve battery efficiency and reduce silver paste consumption, and is also an important topic in the current industrial high-efficiency battery metallization technology research. Screen printing is the core technology for solar cell grid line manufacturing, which directly affects the efficiency of the battery.

[0004] Due to the presence of mesh knots in the screen structure, traditional screen printing technology has problems such as difficulty in grid line thinning, difficulty in slurry passing through the screen, and easy line breakage when printing with a line width below 30μm. The thinning technology is limited by the technical updates of the screen and slurry. In addition, the front silver paste accounts for a large proportion, accounting for between 60% and 70% of the non-silicon cost. The consumption of front printing silver paste accounts for more than 40% of the total production auxiliary material cost. With the development of screen technology, the consumption of silver paste is gradually decreasing. For example, the current step-by-step printing technology can reduce the use of silver paste to a certain extent. However, these current battery metallization technologies still have problems such as large shading area, large resistance, and large amount of silver paste used. Summary of the invention

[0005] Based on this, it is necessary to provide a solar cell and a metallization method thereof to solve the problems of large shading area, high resistance and large amount of silver paste used in the cell metallization technology in the related art.

[0006] In a first aspect, a method for metallizing a solar cell is provided, comprising:

[0007] Providing a silicon substrate, wherein a doping layer is formed on a surface of the silicon substrate;

[0008] A solution of a nano material having a core-shell structure is prepared, wherein the core of the core-shell structure is a metal nanoparticle, and the shell comprises at least: an inorganic nano material contained in glass powder;

[0009] Applying a solution of the nanomaterial having a core-shell structure to a surface of the doping layer away from the silicon substrate to form a liquid film;

[0010] Sintering the liquid film so that the metal nanoparticles are connected into a network structure and connected with the silicon in the doping layer to form a silicon alloy;

[0011] At least two spaced connection lines are formed on a surface of the mesh structure away from the silicon substrate, and the connection lines are used to collect current flowing through the mesh structure.

[0012] Optionally, the metal nanoparticles include: Ag.

[0013] Optionally, the inorganic nanomaterial contained in the glass powder includes one or more of silicon dioxide, titanium dioxide and aluminum oxide.

[0014] Optionally, the particle size of the nanomaterial with a core-shell structure is 200-400 nm, and the particle size of the metal nanoparticles is 2-100 nm.

[0015] Optionally, the solution of the nanomaterial having a core-shell structure is applied to the surface of the doping layer away from the silicon substrate by spin coating or spray coating to form a liquid film.

[0016] Optionally, the concentration of the nanomaterial with a core-shell structure in the solution is 50 wt% to 90 wt%, and the thickness of the liquid film is 0.5 to 5 μm.

[0017] Optionally, the sintering temperature is 650-850° C. and the sintering time is 30-50 seconds.

[0018] In a second aspect, a solar cell prepared by the method described in the first aspect is provided.

[0019] Optionally, the shading area of ​​the mesh structure on the silicon substrate accounts for less than 2%.

[0020] Optionally, the number of the connecting lines is 5 to 20, and the connecting lines are arranged at intervals in a direction perpendicular to the length direction thereof.

[0021] The beneficial effects of the solar cell and the metallization method thereof are as follows:

[0022] By using a nanomaterial with a core-shell structure to replace the silver paste in the related art, and using a solution method to form a liquid film of the nanomaterial with a core-shell structure, the self-assembly characteristics of the nanomaterial with a core-shell structure are utilized, and the metal nanoparticles and the doping layer are connected by sintering to form an electrode pattern with a mesh structure. Then, at least two spaced connecting lines are prepared on the electrode pattern with the mesh structure, so that the current flowing through the mesh structure can be collected, thereby realizing battery metallization; wherein, the electrode pattern with the mesh structure can be regarded as a secondary grid, and the connecting lines are the main grid. In the above preparation process, compared with the secondary grid prepared by screen printing using silver paste in the related art, Metal nanoparticles can contact silicon more effectively, thereby forming a good ohmic contact and reducing resistance. On the other hand, the metal nanoparticles in the electrode pattern of this mesh structure are connected by atomic-level contact, and the line width of the mesh structure can be controlled at the atomic level, which can effectively reduce the shading area and reduce shading losses. For example, compared with the use of silver paste printing in related technologies, the shading area can be reduced to less than 2%. On the other hand, the electrode pattern of this mesh structure is easier to contact with silicon, thereby reducing the amount of silver used. For example, compared with the traditional screen printing silver paste process, the silver consumption can be reduced by more than 30%, greatly reducing the manufacturing cost of crystalline silicon cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A schematic diagram of a process of metallization of a solar cell provided in an embodiment of the present application;

[0024] Figure 2 A schematic diagram of the structure of an electrode pattern formed by metallization of a solar cell provided in an embodiment of the present application. DETAILED DESCRIPTION

[0025] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0026] Unless the context requires otherwise, throughout the specification and claims, the term "including" is to be interpreted as an open, inclusive meaning, that is, "including, but not limited to". In the description of the specification, the terms "one embodiment", "some embodiments", "exemplary embodiments", "exemplarily" or "some examples" and the like are intended to indicate that specific features, structures, materials or characteristics associated with the embodiment or example are included in at least one embodiment or example of the present disclosure. The schematic representation of the above terms does not necessarily refer to the same embodiment or example. In addition, the specific features, structures, materials or characteristics may be included in any one or more embodiments or examples in any appropriate manner.

[0027] Exemplary embodiments are described herein with reference to cross-sectional views and / or plan views that are idealized exemplary drawings. In the drawings, the thickness of layers and regions are exaggerated for clarity. Therefore, variations in shape relative to the drawings due to, for example, manufacturing techniques and / or tolerances are conceivable. Therefore, the exemplary embodiments should not be interpreted as being limited to the shapes of the regions shown herein, but include shape deviations due to, for example, manufacturing. For example, an etched region shown as a rectangle will typically have curved features. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the actual shape of regions of the device, and are not intended to limit the scope of the exemplary embodiments.

[0028] In this document, "for example", "such as", "example", "for example", etc. are used for descriptive purposes, indicating that the previous and subsequent technical solutions are related in terms of the content covered, but should not be understood as limiting the previous technical solution, nor can they be understood as limiting the scope of protection of this document. In this document, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.

[0029] In this article, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel options of "yes" or "no". If there are multiple "options" in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "option" is independent.

[0030] Herein, descriptions such as "optionally contain", "optionally include", etc., mean "contain or not contain". "Optional component X" means component X exists or does not exist, or means containing or not containing the component X.

[0031] In this document, the terms "first", "second", etc. in "the first aspect", "the second aspect", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.

[0032] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0034] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0035] In this document, "at least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc.

[0036] Herein, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers in the numerical interval, including the two endpoint integers of the numerical range, and each integer between the two endpoints, is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.

[0037] In this article, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.

[0038] The fill factor (FF) used in this article refers to the ratio of the actual maximum obtainable power (Pm or Vmp*Jmp) to the theoretical (not actually obtainable) power (Jsc*Voc). Therefore, FF can be determined by the following formula:

[0039] FF=(Vmp*Jmp) / (Jsc*Voc)

[0040] Where Jmp and Vmp represent the current density and voltage at the maximum power point (Pm), which is obtained by changing the resistance in the circuit until J*V is the maximum value; Jsc and Voc represent the short-circuit current and open-circuit voltage, respectively. Fill factor is a key parameter for evaluating solar cells. Commercial solar cells usually have a fill factor of about 60% and above.

[0041] As used herein, open circuit voltage (Voc) is the potential difference between the anode and cathode of a device with no external load connected.

[0042] The power conversion efficiency (PCE) of a solar cell as used herein refers to the percentage of power converted from absorbed light to electrical energy. The power conversion efficiency (PCE) of a solar cell can be measured by the incident light irradiance (E: W / m 2 ) and the surface area of ​​the solar cell (Ac:m 2 ) divided by the maximum power point (Pm). STC usually refers to the temperature of 25℃ and the irradiance of 1000W / m 2 , the spectrum of air quality 1.5 (AM1.5).

[0043] In this article, if there are multiple steps involved in the method flow, unless there is a clear different description in this article, there is no strict order restriction for the execution of these steps, and they can be executed in other orders than described. Moreover, any step can include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn, alternating or simultaneously with other steps or parts of sub-steps or stages of other steps.

[0044] At present, the battery metallization technology mainly adopts screen printing technology. Due to the presence of knots in the screen structure, the traditional screen printing technology has problems such as difficulty in thinning the grid lines, difficulty in passing the slurry through the screen, and easy line breakage when printing with a line width below 30μm. The thinning technology is limited by the technical updates of the screen and slurry. If the mesh material and the slurry are not well matched, the Rs (series resistance) will increase due to the thinning of the grid lines, which will eventually lead to a loss of efficiency. After the slurry is matched with the knotless screen, the high opening rate of the knotless technology is used to greatly increase the amount of ink passing. With the high plasticity of the secondary grid slurry, the aspect ratio of the fine grid lines after printing and sintering can be increased by more than 20%, and the width of the grid line electrode can reach less than 30μm. Even in this case, the shading area of ​​the grid line electrode accounts for about 5%, which limits the increase of short-circuit current, thereby affecting the improvement of battery conversion efficiency.

[0045] Currently, the width of the gate electrode prepared by methods such as light-induced electroplating can reach less than 20μm. Although it can further reduce the shading area of ​​the front gate line and improve the battery conversion efficiency, the high cost of raw materials and equipment for electroplating technology and the extremely complex process limit its application in industrial mass production.

[0046] On the other hand, the positive silver paste accounts for a large proportion of the battery manufacturing cost, accounting for 60% to 70% of the non-silicon cost. The consumption of positive electrode printing silver paste accounts for more than 40% of the total production auxiliary material cost. With the development of screen technology, the consumption of silver paste is gradually decreasing. For example, by the end of 2022, the consumption of single-cell fine grid will be reduced to less than 0.06g, but overall the cost of screen-printed silver paste is still the top priority of battery production costs.

[0047] In the related technology, the step-by-step printing technology is adopted. When printing the main grid, a paste with better conductive properties is selected, and there is no need to penetrate the anti-reflection film. Only the function of current transmission can be realized, avoiding unnecessary recombination and improving the open circuit voltage of the battery. At the same time, since the main grid and the auxiliary grid are printed separately, there is no need to consider the height of the auxiliary grid, and more optimization can be done on the screen to reduce the amount of paste used, thereby reducing the manufacturing cost of solar cells. In terms of the auxiliary grid paste, a paste that can penetrate the anti-reflection film and has good ohmic contact performance is selected to achieve lower contact resistance, and cooperate with the improvement of the resistance of the entire silicon substrate block to effectively improve the efficiency of the battery.

[0048] However, the current battery metallization technologies still have problems such as large shading area, high resistance, large amount of silver paste used, high cost of raw materials and equipment, and complex process.

[0049] Based on the above technical problems, in the first aspect, some embodiments of the present application provide a metallization method for a solar cell, such as Figure 1 and Figure 2 As shown, it includes the following steps S11) to S15):

[0050] S11), providing a silicon substrate, a doping layer is formed on the surface of the silicon substrate.

[0051] Wherein, taking the solar cell as a TOPcon (Tunnel Oxide Passivated Contact solar cell) as an example, the doping layer may be a P-type doping layer or an N-type doping layer.

[0052] Here, taking the solar cell as an N-type TOPcon and metallizing the front surface of the solar cell as an example, the doping layer is a P-type doping layer.

[0053] S12), preparing a solution of nanomaterials having a core-shell structure, wherein the core of the core-shell structure is a metal nanoparticle, and the shell at least comprises: an inorganic nanomaterial contained in the glass powder.

[0054] Among them, the nanomaterial with a core-shell structure is easier to obtain than the silver paste in the related art, and has a higher content of metal nanoparticles. The metal nanoparticles can easily pass through the shell material and contact silicon.

[0055] S13), applying a solution of the nanomaterial having a core-shell structure to the surface of the doping layer away from the silicon substrate to form a liquid film;

[0056] For example, the solution of the nanomaterial may be applied to the surface of the doping layer away from the silicon substrate by spin coating, scraping, spraying, screen printing, etc. to form a liquid film.

[0057] S14), sintering the liquid film so that the metal nanoparticles are connected into a network structure 100 (such as Figure 2 As shown), and forms a silicon alloy with the silicon in the doped layer for connection.

[0058] By sintering the liquid film and utilizing the self-assembly of nanomaterials, the core-shell structured nanomaterials aggregate on the surface of the doping layer. At the same time, during the sintering process, the metal nanoparticles can pass through the shell material to connect into a network structure and contact the doping layer, and a silicon alloy can be formed through sintering and melting.

[0059] Among them, Figure 2 As shown, the black area in the network structure indicates that there are no metal nanoparticles, and the white area is the area where the metal nanoparticles are aggregated and connected, presenting a network structure 100.

[0060] S15), such as Figure 2 As shown, at least two spaced connection lines 200 are formed on a surface of the mesh structure 100 away from the silicon substrate. The connection lines 200 are used to collect the current flowing through the mesh structure 100 .

[0061] In the metallization method of a solar cell provided in an embodiment of the present application, a nanomaterial with a core-shell structure is used to replace the silver paste in the related art, and a solution method is used to form a liquid film of the nanomaterial. The self-assembly characteristics of the nanomaterial with a core-shell structure are utilized to connect the metal nanoparticles and the doping layer through sintering to form an electrode pattern with a mesh structure. Then, only at least two spaced connecting lines are prepared on the electrode pattern with the mesh structure to collect the current flowing through the mesh structure, thereby realizing battery metallization. Among them, the electrode pattern with the mesh structure can be regarded as a secondary grid, and the connecting lines are the main grid. In the above preparation process, the silver paste is used to form a liquid film of the nanomaterial by screen printing in the related art. Compared with brush-prepared sub-grids, metal nanoparticles can contact silicon more effectively, thereby forming good ohmic contact and reducing resistance; on the other hand, the metal nanoparticles in the electrode pattern of this mesh structure are connected by atomic-level contact, and the line width of the mesh structure can be controlled at the atomic level, thereby effectively reducing the shading area and reducing shading losses. For example, compared with the related technology of using silver paste printing, the shading area can be reduced to less than 2%; on another hand, the electrode pattern of this mesh structure is easier to contact with silicon, thereby reducing the amount of silver used. For example, compared with the traditional screen printing silver paste process, the silver consumption can be reduced by more than 30%, greatly reducing the manufacturing cost of crystalline silicon cells.

[0062] In addition, the above-mentioned nanomaterials with core-shell structure are easy to obtain, low in cost, and simple in preparation method. Compared with the metallization of the battery by electroplating, the cost of raw materials and equipment can be effectively reduced.

[0063] The specific material of the metal nanoparticles is not limited. For example, the metal nanoparticles may be precious metal particles, such as silver, gold, platinum, etc.

[0064] In some embodiments, the metal nanoparticles may include: Ag.

[0065] In these embodiments, silver can be used as the electrode material. Compared with the related art of using silver paste printing to form gate lines, the amount of silver paste can be saved. Moreover, since the organic binder and other components in the silver paste are discarded, the metallic silver can be more conducive to passing through the shell material and contacting silicon, thereby forming a better ohmic contact with silicon. At the same time, different from the principle of using silver paste printing to form gate lines, the silver electrode can be prepared by self-assembly.

[0066] In some embodiments, the inorganic nanomaterials contained in the glass powder include one or more of silicon dioxide, titanium dioxide, and aluminum oxide.

[0067] In some embodiments, the particle size of the nanomaterial with a core-shell structure is 200-400 nm, and the particle size of the metal nanoparticles is 2-100 nm.

[0068] In these embodiments, by limiting the particle size of the nanomaterial with a core-shell structure and the particle size of the metal nanoparticles within the above ranges, a metal nanoparticle network aggregation structure can be more effectively formed by self-assembly, thereby obtaining a finer metal grid line electrode.

[0069] The method for obtaining the nanomaterial with a core-shell structure is not specifically limited. The nanomaterial with a core-shell structure can be obtained through commercial channels or prepared.

[0070] In some embodiments, preparing a solution of a nanomaterial having a core-shell structure may include:

[0071] Nanomaterials with core-shell structure were prepared by sol-gel method;

[0072] The nano material with a core-shell structure is dissolved in an organic solvent to prepare a solution of the nano material with a core-shell structure.

[0073] Among them, taking Ag@SiO2 as an example of a nanomaterial with a core-shell structure, the raw materials used in the sol-gel method may include: a silane coupling agent, silver nitrate and tetraethyl orthosilicate (TEOS), and the nanomaterial can be prepared by hydrolyzing TEOS.

[0074] In some embodiments, the raw materials used in the sol-gel method may further include ammonia water, which can promote the hydrolysis of TEOS.

[0075] In some embodiments, the organic solvent may be an alcohol solvent, such as methanol, ethanol, etc.

[0076] In some embodiments, a solution of the nanomaterial having a core-shell structure is applied to the surface of the doping layer away from the silicon substrate by spin coating or spray coating to form a liquid film.

[0077] In these embodiments, spin coating or spray coating can be used to evenly coat the solution of the nanomaterial with a core-shell structure on the surface of the doping layer, thereby facilitating the formation of a more regular network structure and reducing the loss of the network structure.

[0078] In some embodiments, the concentration of the nanomaterial having a core-shell structure in the solution is 50 wt % to 90 wt %, and the thickness of the liquid film is 0.5 to 5 μm.

[0079] In these embodiments, it is possible to ensure that a relatively regular mesh structure is formed and reduce the loss of the mesh structure.

[0080] In some embodiments, the sintering temperature is 650-850° C. and the sintering time is 30-50 seconds.

[0081] It should be noted that the above-mentioned applying the solution of the nanomaterial with a core-shell structure to the surface of the doping layer away from the silicon substrate means directly applying the solution of the nanomaterial with a core-shell structure to the surface of the doping layer so that the solution of the nanomaterial with a core-shell structure is in direct contact with the doping layer. At this time, it is convenient for the nanomaterial with a core-shell structure to directly react with the silicon in the doping layer.

[0082] In other embodiments, before applying the solution of the nanomaterial having a core-shell structure to the surface of the doping layer away from the silicon substrate, the method may further include: forming a passivation layer on the surface of the doping layer away from the silicon substrate.

[0083] At this time, due to the existence of the passivation layer, the nanomaterial with a core-shell structure needs to ablate the passivation layer before reacting with the silicon in the doping layer. The ohmic contact effect finally formed is not as good as the ohmic contact effect formed by the direct reaction above.

[0084] In some embodiments, the number of the connecting lines is 5 to 20, and the connecting lines are arranged at intervals in a direction perpendicular to the length direction thereof.

[0085] In these embodiments, the connecting wires may be prepared by screen printing.

[0086] In a second aspect, some embodiments of the present application provide a solar cell prepared by the method described in the first aspect.

[0087] The solar cell comprises a first conductive layer and a second conductive layer, wherein the first conductive layer comprises metal nanoparticles, the metal nanoparticles are connected into a mesh structure and form a silicon alloy with the silicon of the doped layer to achieve connection, and the second conductive layer comprises at least two spaced connecting wires, which are used to collect current flowing through the mesh structure.

[0088] Among them, the first conductive layer can be prepared by self-assembly of nanomaterials with a core-shell structure, and the connecting wire can be prepared by screen printing, which can effectively reduce the use of silver paste. In the preparation process, compared with the preparation of the sub-grid by screen printing with silver paste in the related technology, the metal nanoparticles can contact with silicon more effectively, thereby forming a good ohmic contact and reducing resistance. The metal nanoparticles in the electrode pattern of this mesh structure are connected by atomic-level contact, and the line width of the mesh structure can be controlled at the atomic level, thereby effectively reducing the shading area and reducing the shading loss.

[0089] In some embodiments, the mesh structure accounts for less than 2% of the light shielding area on the silicon substrate.

[0090] In these embodiments, the shading area is greatly reduced, thereby reducing shading losses.

[0091] For example, in some examples, the mesh structure accounts for 1% to 2% of the light shielding area on the silicon substrate.

[0092] In some embodiments, the number of the connecting lines is 5 to 20, and the connecting lines are arranged at intervals along a direction perpendicular to the length direction thereof.

[0093] In these embodiments, the current collection efficiency can be effectively improved and the series resistance can be reduced.

[0094] In order to objectively evaluate the technical effects of the embodiments of the present application, the present application will be described in detail and exemplarily through the following embodiments and comparative examples.

[0095] In the following examples and comparative examples, all raw materials can be purchased commercially, and in order to maintain the reliability of the experiment, the raw materials used in the following examples and comparative examples have the same physical and chemical parameters or are prepared by the same processing method.

[0096] Example 1

[0097] The method for preparing the solar cell in Example 1 is as follows:

[0098] Step 1), silver nitrate methanol solution and TSD (N-(2-Aminoethyl)aminopropyl]trimethoxysilane), N-(2-aminoethyl)-aminopropyltrimethoxysilane) methanol solution are mixed in a certain proportion, and the mixed solution is added to a methanol solution containing a certain proportion of TEOS (Tetraethoxysilane, also known as tetraethyl silicate) and ammonia water;

[0099] Step 2), adding a certain concentration of formaldehyde solution to the mixed solution of step 1) and stirring at a constant temperature to obtain a solution of Ag@SiO2 composite particles; wherein the concentration of the silver nitrate methanol solution is 0.01 mol / L, the constant temperature of the mixed solution is 20°C, and the constant temperature stirring time is 20 minutes; the particle size of the obtained composite particles is 200 nm, wherein the particle size of the doped silver is 2 nm;

[0100] Step 3), after preparing the suede structure, PN junction and passivation layer on the N-type silicon wafer, a solution of Ag@SiO2 composite particles is coated on the surface of the silicon wafer by spin coating; the thickness of the spin coating is 0.5 μm;

[0101] Step 4), printing low-temperature main grid silver paste as the main grid electrode according to the main grid welding pattern on the surface of the above-mentioned Ag@SiO2 composite particles; then putting it into a sintering furnace for electrode sintering, wherein the sintering temperature is 650°C, the time is 50s, and the number of main grid electrodes is 5.

[0102] Example 2

[0103] The preparation method of the solar cell in Example 2 is as follows:

[0104] Step 1), mixing silver nitrate methanol solution and TSD methanol solution in a certain proportion, and adding the mixed solution into a methanol solution containing TEOS and ammonia water in a certain ratio;

[0105] Step 2), adding a certain concentration of formaldehyde solution to the mixed solution of step 1) and stirring at a constant temperature to obtain a solution of Ag@SiO2 composite particles; wherein the concentration of the silver nitrate methanol solution is 0.1 mol / L, the constant temperature of the mixed solution is 50°C, and the constant temperature stirring time is 200 min; the particle size of the obtained composite particles is 400 nm, wherein the particle size of the doped silver is 100 nm;

[0106] Step 3), after preparing the suede structure, PN junction and passivation layer on the N-type silicon wafer, a solution of Ag@SiO2 composite particles is coated on the surface of the silicon wafer by spraying; the thickness of the sprayed layer is 5 μm;

[0107] Step 4), printing low-temperature main grid silver paste as the main grid electrode according to the main grid welding pattern on the surface of the Ag@SiO2 composite particles coated above; then putting it into the sintering furnace for electrode sintering, wherein the sintering temperature is 700°C, the time is 40s, and the number of main grid electrodes is 20.

[0108] Example 3

[0109] The preparation method of the solar cell in Example 3 is as follows:

[0110] Step 1), mixing silver nitrate methanol solution and TSD methanol solution in a certain proportion, and adding the mixed solution into a methanol solution containing TEOS and ammonia water in a certain ratio;

[0111] Step 2), adding a certain concentration of formaldehyde solution to the mixed solution of step 1) and stirring at a constant temperature to obtain a solution of Ag@SiO2 composite particles; wherein the concentration of the silver nitrate methanol solution is 0.05 mol / L, the constant temperature of the mixed solution is 30°C, and the constant temperature stirring time is 100 min; the particle size of the obtained composite particles is 300 nm, wherein the particle size of the doped silver is 50 nm;

[0112] Step 3), after preparing the suede structure, PN junction and passivation layer on the N-type silicon wafer, a solution of Ag@SiO2 composite particles is coated on the surface of the silicon wafer by spraying; the thickness of the sprayed layer is 3 μm;

[0113] Step 4), printing low-temperature main grid silver paste as the main grid electrode according to the main grid welding pattern on the surface of the above-mentioned Ag@SiO2 composite particles; then putting it into a sintering furnace for electrode sintering, wherein the sintering temperature is 850°C, the time is 30s, and the number of main grid electrodes is 10.

[0114] Comparative Example 1

[0115] The preparation method of the solar cell in Comparative Example 1 is as follows:

[0116] After preparing a suede structure, a PN junction and a passivation layer on an N-type silicon wafer, the secondary gate and the main gate electrodes are prepared by screen printing silver paste and sintering at 650°C for 50s. The number of the main gate electrodes is 5.

[0117] Test Case

[0118] By testing the open circuit voltage Voc, short circuit current Jsc, fill factor FF and power conversion efficiency PCE of Examples 1 to 3 and Comparative Example 1, the test results are shown in Table 1 below.

[0119] Table 1

[0120] Test items PCE(%) <![CDATA[Jsc(mA / cm 2 )]]> Voc(V) FF(%) Comparative Example 1 25.42 41.5 0.7176 85.28 Example 1 25.41 41.6 0.7188 85.04 Example 2 25.68 41.6 0.7159 86.22 Example 3 25.74 41.7 0.7164 86.26

[0121] It can be seen from Table 1 that the solar cell provided in the embodiment of the present application can reduce silver consumption and increase short-circuit current, while the efficiency is almost the same as or higher than that of Comparative Example 1.

[0122] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0123] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for metallizing a solar cell, characterized in that: include: Providing a silicon substrate, wherein a doping layer is formed on a surface of the silicon substrate; Dissolving a nanomaterial having a core-shell structure in an organic solvent to prepare a solution of the nanomaterial having a core-shell structure, wherein the core of the core-shell structure is a metal nanoparticle, and the shell at least comprises: an inorganic nanomaterial contained in glass powder; Applying a solution of the nanomaterial having a core-shell structure to a surface of the doping layer away from the silicon substrate to form a liquid film; Sintering the liquid film so that the metal nanoparticles are connected into a network structure and connected with the silicon in the doping layer to form a silicon alloy; At least two spaced connection lines are formed on a surface of the mesh structure away from the silicon substrate, wherein the connection lines are used to collect current flowing through the mesh structure; Wherein, the light shielding area of ​​the mesh structure on the silicon substrate accounts for less than 2%.

2. The method according to claim 1, characterized in that The metal nanoparticles include: Ag.

3. The method according to claim 1, characterized in that The inorganic nanomaterials contained in the glass powder include one or more of silicon dioxide, titanium dioxide and aluminum oxide.

4. The method according to any one of claims 1 to 3, characterized in that: The particle size of the nano material with a core-shell structure is 200-400 nm, and the particle size of the metal nanoparticles is 2-100 nm.

5. The method according to any one of claims 1 to 3, characterized in that: The solution of the nano material with the core-shell structure is applied to the surface of the doping layer away from the silicon substrate by spin coating or spray coating to form a liquid film.

6. The method according to claim 5, characterized in that The concentration of the nano material with a core-shell structure in the solution is 50wt% to 90wt%, and the thickness of the liquid film is 0.5 to 5μm.

7. The method according to any one of claims 1 to 3, characterized in that: The sintering temperature is 650-850° C. and the sintering time is 30-50 seconds.

8. A solar cell prepared by the method according to any one of claims 1 to 7.

9. The solar cell according to claim 8, characterized in that The number of the connecting lines is 5 to 20 and they are arranged at intervals in a direction perpendicular to the length direction thereof.

Citation Information

Patent Citations

  • Photovoltaic cells having a back side passivation layer

    CN105190905A

  • Front electrode for battery

    CN113113170A