Nylon film with puncture resistance and high surface wetting tension and preparation method and application thereof
By adding cross-linking-wetting dual-effect modifier and auxiliary cross-linking agent to the nylon film and performing low-power ultraviolet cross-linking, the problem of degradation of performance of nylon film after moisture is solved, achieving high puncture strength and high The surface wetting tension improves the overall performance of aluminum-plastic composite film for lithium-ion batteries.
Patent Information
- Application Number
- CN202410040914.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-01-11
AI Technical Summary
The nylon film of existing aluminum-plastic composite film for lithium-ion batteries has reduced barrier properties, mechanical properties and peel strength of aluminum foil after moisture. Radiation crosslinking and high-power ultraviolet crosslinking methods are prone to molecular degradation and surface oxidation, which is difficult to both. With high puncture strength and high surface wetting tension.
On the basis of not changing the bidirectional stretched nylon film production process, cross-linking-wetting dual-effect modifier and auxiliary cross-linking agent are added to the nylon film, and puncture-resistant and high-surface are prepared by low-power ultraviolet light cross-linking. The nylon film with wetting tension includes 87 to 94 parts of nylon particles, 4 to 8 parts of cross-linking-wetting dual-effect modifier, and 1 to 2 parts of auxiliary cross-linking agent tetradimethylvinylsiloxy The silane, 0.5 to 1 part of the photoinitiator 2-hydroxy-2-methylphenylacetone and 0.5 to 2 parts of nano-silica are subjected to low-power ultraviolet light irradiation.
The high puncture strength and high surface wetting tension of the nylon film are achieved, and the molecular degradation and crystallinity reduction caused by radiation crosslinking and high-power ultraviolet crosslinking are avoided. The aluminum plastic can be combined with aluminum foil without corona treatment. The composite film has thinner thickness and higher tensile strength, puncture strength and peel strength.
Smart Images

Figure CN117965023B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thin films, and in particular relates to a nylon film with high surface wetting tension and puncture resistance, and a preparation method and application thereof. Background Art
[0002] The existing aluminum-plastic composite film for lithium-ion batteries usually uses stretched nylon as a protective layer, aluminum foil as a core layer, and polypropylene as a heat-sealing layer. The protective layer nylon has a polar molecular structure and strong hygroscopicity. After being damp, the barrier properties, mechanical properties, and peel strength of the nylon film with the aluminum foil are reduced, and even delamination occurs. The use environment of lithium-ion batteries is complex, and the aluminum-plastic composite film needs to have good performance in various environmental conditions.
[0003] In order to improve the puncture strength and tensile strength of nylon film, the modification methods of radiation crosslinking and ultraviolet light crosslinking are mainly used. Radiation crosslinking can significantly increase the crosslinking degree of nylon molecules, but it will affect the molecular crystallization, resulting in molecular chain breakage and degradation, and the radiation dose and time need to be strictly controlled. The ultraviolet light crosslinking process requires the light source to have a high power density, which can easily lead to oxidation of the film surface and reduced mechanical strength. In addition, the surface wetting tension of nylon film is generally 30 to 46 mN / m. In order to ensure the high peel strength of the composite of nylon and aluminum foil, the nylon needs to be corona treated. On the basis of not changing the production process of biaxially stretched nylon film, the present invention adds a crosslinking-wetting dual-effect modifier and an auxiliary crosslinking agent to the nylon film, and obtains a nylon film with both high puncture strength and high surface wetting tension through low-power ultraviolet crosslinking. Summary of the invention
[0004] Aiming at the shortcomings of the existing biaxially stretched nylon film for aluminum foil composite, the present invention provides a nylon film with high surface wetting tension and puncture resistance, and a preparation method and application thereof.
[0005] The present invention provides a puncture-resistant nylon film with high surface wetting tension, characterized in that, based on weight, the film comprises 87 to 94 parts of nylon particles, 4 to 8 parts of a cross-linking-wetting dual-effect modifier, 1 to 2 parts of an auxiliary cross-linking agent tetrakis dimethylvinylsiloxysilane, 0.5 to 1 part of a photoinitiator 2-hydroxy-2-methylpropiophenone, and 0.5 to 2 parts of nano silicon dioxide; the cross-linking-wetting dual-effect modifier is a mixture of chemical formula 1, chemical formula 2, chemical formula 3 and chemical formula 4.
[0006] Preferably, the nylon particles are composed of one or a combination of more than one of nylon 6, nylon 66, nylon 610, nylon 10 and nylon 12.
[0007] The method for preparing a puncture-resistant and high-surface wetting tension nylon film is characterized in that it comprises the following steps: step 1, preparing a cross-linking-wetting dual-effect modifier; step 2, preparing modified nylon particles; step 3, stretching the nylon film; step 4, preparing the nylon film;
[0008] In step 1, 5 g of aluminum lactate and 2 mL of triethylamine are dissolved in 100 mL of dichloromethane, the temperature is lowered to 5° C., 2 to 4 g of acryloyl chloride is slowly added dropwise, and after reacting for 12 hours, the remaining acryloyl chloride, triethylamine and dichloromethane are removed by rotary evaporation, and triethylamine hydrochloride is removed by column chromatography to obtain a cross-linking-wetting dual-effect modifier;
[0009] In step 2, nylon particles, a cross-linking-wetting dual-effect modifier, an auxiliary cross-linking agent, tetradimethylvinylsiloxysilane, a photoinitiator, 2-hydroxy-2-methylpropiophenone, and nano-silica are added to a twin-screw extruder in proportion for blending and granulation, and the three-zone temperatures are 140° C., 180° C., and 170° C. to obtain modified nylon particles;
[0010] In step 3, the modified nylon particles are added into a casting machine for extrusion casting, and the cast sheet is synchronously biaxially stretched to obtain a biaxially stretched nylon film, the stretching temperature is 140-170° C., the transverse stretching ratio is 1.6-1.9, and the longitudinal stretching ratio is 1.8-2.8;
[0011] In step 4, the biaxially stretched nylon film is irradiated with low-power ultraviolet light, with a wavelength range of 350 to 400 nm, a power of 10 to 25 W, and an irradiation time of 10 to 30 seconds to obtain a nylon film with puncture resistance and high surface wetting tension.
[0012] A composite polyurethane adhesive with a thickness of 5 to 20 μm is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a nylon film with puncture resistance and high surface wetting tension is pressed onto the adhesive, and an aluminum-plastic composite film for lithium-ion batteries is obtained after curing.
[0013] Compared with the prior art, the present invention first prepares a cross-linking-curing dual-effect modifier, melt-blends it and adds it to nylon, then performs casting, biaxial stretching and low-power ultraviolet light cross-linking to obtain a biaxially stretched nylon film for aluminum foil composite. The process method can effectively avoid the degradation of nylon molecules and the reduction of crystallinity caused by radiation cross-linking and high-power ultraviolet light cross-linking, and has high surface wetting tension, and can be composited with aluminum foil with high peel strength without corona treatment. The aluminum-plastic composite film for ion batteries obtained by composite the puncture-resistant and high surface wetting tension nylon film of the present invention with aluminum foil / polypropylene is thinner than the commercially available aluminum-plastic composite film for lithium ion batteries, and has higher tensile strength, puncture strength and peel strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1is a system flow chart of the present invention;
[0015] Figure 2 is the chemical formula 1 in the present invention;
[0016] Figure 3 It is the chemical formula 2 in the present invention;
[0017] Figure 4 It is the chemical formula 3 in the present invention;
[0018] Figure 5 It is the chemical formula 4 in the present invention. DETAILED DESCRIPTION
[0019] To facilitate understanding of the present invention, the present invention will be described more comprehensively below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings, but the present invention can be implemented in different forms and is not limited to the embodiments described in the text. On the contrary, these embodiments are provided to make the content disclosed in the present invention more thorough and comprehensive.
[0020] The puncture-resistant and high-surface wetting tension nylon film is characterized in that, by weight, it comprises 87 to 94 parts of nylon particles, 4 to 8 parts of a cross-linking-wetting dual-effect modifier, 1 to 2 parts of an auxiliary cross-linking agent tetrakis dimethylvinylsiloxysilane, 0.5 to 1 part of a photoinitiator 2-hydroxy-2-methylpropiophenone, and 0.5 to 2 parts of nano-silicon dioxide; the cross-linking-wetting dual-effect modifier is a mixture of chemical formula 1, chemical formula 2, chemical formula 3, and chemical formula 4.
[0021] Preferably, the nylon particles are composed of one or a combination of more than one of nylon 6, nylon 66, nylon 610, nylon 10 and nylon 12.
[0022] The method for preparing a puncture-resistant and high-surface wetting tension nylon film is characterized in that it comprises the following steps: step 1, preparing a cross-linking-wetting dual-effect modifier; step 2, preparing modified nylon particles; step 3, stretching the nylon film; step 4, preparing the nylon film;
[0023] In step 1, 5 g of aluminum lactate and 2 mL of triethylamine are dissolved in 100 mL of dichloromethane, the temperature is lowered to 5° C., 2 to 4 g of acryloyl chloride is slowly added dropwise, and after reacting for 12 hours, the remaining acryloyl chloride, triethylamine and dichloromethane are removed by rotary evaporation, and triethylamine hydrochloride is removed by column chromatography to obtain a cross-linking-wetting dual-effect modifier;
[0024] In step 2, nylon particles, a cross-linking-wetting dual-effect modifier, an auxiliary cross-linking agent, tetradimethylvinylsiloxysilane, a photoinitiator, 2-hydroxy-2-methylpropiophenone, and nano-silica are added to a twin-screw extruder in proportion for blending and granulation, and the three-zone temperatures are 140° C., 180° C., and 170° C. to obtain modified nylon particles;
[0025] In step 3, the modified nylon particles are added into a casting machine for extrusion casting, and the cast sheet is synchronously biaxially stretched to obtain a biaxially stretched nylon film, the stretching temperature is 140-170° C., the transverse stretching ratio is 1.6-1.9, and the longitudinal stretching ratio is 1.8-2.8;
[0026] In step 4, the biaxially stretched nylon film is irradiated with low-power ultraviolet light, with a wavelength range of 350 to 400 nm, a power of 10 to 25 W, and an irradiation time of 10 to 30 seconds to obtain a nylon film with puncture resistance and high surface wetting tension.
[0027] A composite polyurethane adhesive with a thickness of 5 to 20 μm is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a nylon film with puncture resistance and high surface wetting tension is pressed onto the adhesive, and an aluminum-plastic composite film for lithium-ion batteries is obtained after curing.
[0028] Example 1
[0029] This embodiment provides a method for preparing a nylon film with puncture resistance and high surface wetting tension, which is as follows:
[0030] (1) 5 g of aluminum lactate and 2 mL of triethylamine were dissolved in 100 mL of dichloromethane, the temperature was lowered to 5° C., 2 g of acryloyl chloride was slowly added dropwise, and after reacting for 12 hours, the remaining acryloyl chloride, triethylamine and dichloromethane were removed by rotary evaporation, and triethylamine hydrochloride was removed by column chromatography to obtain a cross-linking-wetting dual-effect modifier;
[0031] (2) adding 94 parts of nylon 66 particles, 4 parts of a cross-linking-wetting dual-effect modifier, 1 part of an auxiliary cross-linking agent tetradimethylvinylsiloxysilane, 0.5 parts of a photoinitiator 2-hydroxy-2-methylpropiophenone and 0.5 parts of nano-silicon dioxide into a twin-screw extruder for blending and granulation, with the three-zone temperatures at 140° C., 180° C. and 170° C. to obtain modified nylon particles;
[0032] (3) adding the modified nylon particles into a casting machine for extrusion casting, and synchronously biaxially stretching the cast sheet to obtain a biaxially stretched nylon film, the stretching temperature is 170° C., the transverse stretching ratio is 1.9, and the longitudinal stretching ratio is 2.8;
[0033] (4) The biaxially stretched nylon film was irradiated with low-power ultraviolet light at a wavelength of 350 nm, a power of 25 W, and an irradiation time of 30 s to obtain a nylon film with puncture resistance and high surface wetting tension.
[0034] A 5 μm thick composite polyurethane adhesive is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a puncture-resistant and high surface wetting tension nylon film is pressed onto the adhesive, and after curing, an aluminum-plastic composite film for lithium-ion batteries is obtained.
[0035] Example 2
[0036] This embodiment provides a method for preparing a nylon film with puncture resistance and high surface wetting tension, which is as follows:
[0037] (1) 5 g of aluminum lactate and 2 mL of triethylamine were dissolved in 100 mL of dichloromethane, the temperature was lowered to 5° C., 4 g of acryloyl chloride was slowly added dropwise, and after reacting for 12 hours, the remaining acryloyl chloride, triethylamine and dichloromethane were removed by rotary evaporation, and triethylamine hydrochloride was removed by column chromatography to obtain a cross-linking-wetting dual-effect modifier;
[0038] (2) adding 90 parts of nylon 10 particles, 8 parts of a cross-linking-wetting dual-effect modifier, 1 part of an auxiliary cross-linking agent tetradimethylvinylsiloxysilane, 0.5 parts of a photoinitiator 2-hydroxy-2-methylpropiophenone and 0.5 parts of nano-silica into a twin-screw extruder for blending and granulation, with the three-zone temperatures at 140° C., 180° C. and 170° C. to obtain modified nylon particles;
[0039] (3) adding the modified nylon particles into a casting machine for extrusion casting, and synchronously biaxially stretching the cast sheet to obtain a biaxially stretched nylon film, wherein the stretching temperature is 140° C., the transverse stretching ratio is 1.6, and the longitudinal stretching ratio is 1.8;
[0040] (4) The biaxially stretched nylon film was irradiated with low-power ultraviolet light at a wavelength of 400 nm, a power of 28 W, and an irradiation time of 20 s to obtain a nylon film with puncture resistance and high surface wetting tension.
[0041] The composite polyurethane adhesive with a thickness of 8 μm is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a nylon film with puncture resistance and high surface wetting tension is pressed on the adhesive, and after curing, an aluminum-plastic composite film for lithium-ion batteries is obtained.
[0042] Example 3
[0043] This embodiment provides a method for preparing a nylon film with puncture resistance and high surface wetting tension, which is as follows:
[0044] (1) 5 g of aluminum lactate and 2 mL of triethylamine were dissolved in 100 mL of dichloromethane, the temperature was lowered to 5° C., 3 g of acryloyl chloride was slowly added dropwise, and after reacting for 12 hours, the remaining acryloyl chloride, triethylamine and dichloromethane were removed by rotary evaporation, and triethylamine hydrochloride was removed by column chromatography to obtain a cross-linking-wetting dual-effect modifier;
[0045] (2) adding 87 parts of nylon 12 particles, 8 parts of a cross-linking-wetting dual-effect modifier, 2 parts of an auxiliary cross-linking agent tetradimethylvinylsiloxysilane, 1 part of a photoinitiator 2-hydroxy-2-methylpropiophenone and 2 parts of nano-silica into a twin-screw extruder for blending and granulation, with the three-zone temperatures at 140° C., 180° C. and 170° C. to obtain modified nylon particles;
[0046] (3) adding the modified nylon particles into a casting machine for extrusion casting, and synchronously biaxially stretching the cast sheet to obtain a biaxially stretched nylon film, the stretching temperature is 150° C., the transverse stretching ratio is 1.8, and the longitudinal stretching ratio is 2.2;
[0047] (4) The biaxially stretched nylon film was irradiated with low-power ultraviolet light at a wavelength of 380 nm, a power of 18 W, and an irradiation time of 10 s to obtain a nylon film with puncture resistance and high surface wetting tension.
[0048] A 10 μm thick composite polyurethane adhesive is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a puncture-resistant and high surface wetting tension nylon film is pressed onto the adhesive, and after curing, an aluminum-plastic composite film for lithium-ion batteries is obtained.
[0049] Example 4
[0050] This embodiment provides a method for preparing a nylon film with puncture resistance and high surface wetting tension, which is as follows:
[0051] (1) 5 g of aluminum lactate and 2 mL of triethylamine were dissolved in 100 mL of dichloromethane, the temperature was lowered to 5° C., 4 g of acryloyl chloride was slowly added dropwise, and after reacting for 12 hours, the remaining acryloyl chloride, triethylamine and dichloromethane were removed by rotary evaporation, and triethylamine hydrochloride was removed by column chromatography to obtain a cross-linking-wetting dual-effect modifier;
[0052] (2) adding 89 parts of nylon 6 particles, 7 parts of a cross-linking-wetting dual-effect modifier, 2 parts of an auxiliary cross-linking agent tetradimethylvinylsiloxysilane, 1 part of a photoinitiator 2-hydroxy-2-methylpropiophenone and 1 part of nano-silica into a twin-screw extruder for blending and granulation, with the three-zone temperatures at 140° C., 180° C. and 170° C. to obtain modified nylon particles;
[0053] (3) adding the modified nylon particles into a casting machine for extrusion casting, and synchronously biaxially stretching the cast sheet to obtain a biaxially stretched nylon film, wherein the stretching temperature is 160° C., the transverse stretching ratio is 1.7, and the longitudinal stretching ratio is 2.2;
[0054] (4) The biaxially stretched nylon film was irradiated with low-power ultraviolet light at a wavelength of 390 nm, a power of 23 W, and an irradiation time of 28 s to obtain a nylon film with puncture resistance and high surface wetting tension.
[0055] A 15 μm thick composite polyurethane adhesive is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a puncture-resistant and high surface wetting tension nylon film is pressed onto the adhesive, and after curing, an aluminum-plastic composite film for lithium-ion batteries is obtained.
[0056] Example 5
[0057] This embodiment provides a method for preparing a nylon film with puncture resistance and high surface wetting tension, which is as follows:
[0058] (1) 5 g of aluminum lactate and 2 mL of triethylamine were dissolved in 100 mL of dichloromethane, the temperature was lowered to 5° C., 4 g of acryloyl chloride was slowly added dropwise, and after reacting for 12 hours, the remaining acryloyl chloride, triethylamine and dichloromethane were removed by rotary evaporation, and triethylamine hydrochloride was removed by column chromatography to obtain a cross-linking-wetting dual-effect modifier;
[0059] (2) adding 50 parts of nylon 66 and 39 parts of nylon 12 particles, 6 parts of a cross-linking-wetting dual-effect modifier, 2 parts of an auxiliary cross-linking agent tetradimethylvinylsiloxysilane, 0.8 parts of a photoinitiator 2-hydroxy-2-methylpropiophenone and 2.2 parts of nano-silica into a twin-screw extruder for blending and granulation, with the three-zone temperatures at 140° C., 180° C. and 170° C. to obtain modified nylon particles;
[0060] (3) adding the modified nylon particles into a casting machine for extrusion casting, and synchronously biaxially stretching the cast sheet to obtain a biaxially stretched nylon film, wherein the stretching temperature is 160° C., the transverse stretching ratio is 1.6, and the longitudinal stretching ratio is 1.9;
[0061] (4) The biaxially stretched nylon film was irradiated with low-power ultraviolet light at a wavelength of 400 nm, a power of 25 W, and an irradiation time of 30 s to obtain a nylon film with puncture resistance and high surface wetting tension.
[0062] A 20 μm thick composite polyurethane adhesive is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a puncture-resistant and high surface wetting tension nylon film is pressed onto the adhesive, and after curing, an aluminum-plastic composite film for lithium-ion batteries is obtained.
[0063] Comparative Example 1
[0064] (1) adding 90 parts of nylon 10 particles, 6 parts of crosslinking agent triallyl cyanurate, 2 parts of photoinitiator benzophenone and 2 parts of nano-silicon dioxide into a twin-screw extruder for blending and granulation, with the temperatures in three zones being 140° C., 180° C. and 170° C., to obtain modified nylon particles;
[0065] (2) adding the modified nylon particles into a casting machine for extrusion casting, and synchronously biaxially stretching the cast sheet to obtain a biaxially stretched nylon film, wherein the stretching temperature is 160° C., the transverse stretching ratio is 1.6, and the longitudinal stretching ratio is 1.9;
[0066] (3) The biaxially stretched nylon film was irradiated with ultraviolet light at a wavelength of 365 nm, a power of 2000 W, and an irradiation time of 10 s to obtain a nylon film.
[0067] A 15 μm thick composite polyurethane adhesive is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then the nylon film is pressed onto the adhesive, and the aluminum-plastic composite film is obtained after curing.
[0068] Comparative Example 2
[0069] 1) adding 94 parts of nylon 10 particles, 4 parts of crosslinking agent divinylbenzene, 1 part of photoinitiator benzoin dimethyl ether and 1 part of nano-silicon dioxide into a twin-screw extruder for blending and granulation, with three-zone temperatures of 140° C., 180° C. and 170° C. to obtain modified nylon particles;
[0070] (2) adding the modified nylon particles into a casting machine for extrusion casting, and synchronously biaxially stretching the cast sheet to obtain a biaxially stretched nylon film, wherein the stretching temperature is 170° C., the transverse stretching ratio is 1.9, and the longitudinal stretching ratio is 2.8;
[0071] (3) The biaxially stretched nylon film was irradiated with ultraviolet light at a wavelength of 385 nm, a power of 1000 W, and an irradiation time of 20 s to obtain a nylon film.
[0072] A 20 μm thick composite polyurethane adhesive is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then the nylon film is pressed onto the adhesive, and the aluminum-plastic composite film is obtained after curing.
[0073] The properties of the nylon films in the examples and comparative examples and the commercially available nylon films were tested according to the requirements of GB / T 20218-2021. The properties of the aluminum-plastic composite films in the examples and comparative examples and the commercially available aluminum-plastic composite films for lithium-ion batteries were tested according to the requirements of GB / T 10004-2008.
[0074] Table 1 Comparison of performance of examples, comparative examples and commercially available films
[0075]
Claims
1. A nylon film with puncture resistance and high surface wetting tension, characterized in that: In parts by weight, it comprises 87 to 94 parts of nylon particles, 4 to 8 parts of a cross-linking-wetting dual-effect modifier, 1 to 2 parts of an auxiliary cross-linking agent, tetradimethylvinylsiloxysilane, 0.5 to 1 part of a photoinitiator, 2-hydroxy-2-methylpropiophenone, and 0.5 to 2 parts of nano silicon dioxide; the cross-linking-wetting dual-effect modifier is: ; Chemical formula 1, ; Chemical formula 2: ; Chemical formula 3 and ; A mixture of chemical formula 4; The preparation method of the cross-linking-wetting dual-effect modifier is as follows: 5g of aluminum lactate and 2mL of triethylamine are dissolved in 100mL of dichloromethane, the temperature is lowered to 5°C, 2-4g of acryloyl chloride is slowly added dropwise, and after reacting for 12h, the remaining acryloyl chloride, triethylamine and dichloromethane are removed by rotary evaporation, and triethylamine hydrochloride is removed by column chromatography to obtain the cross-linking-wetting dual-effect modifier.
2. The puncture-resistant and high surface wetting tension nylon film according to claim 1, characterized in that: The nylon particles are composed of one or a combination of more than one of nylon 6, nylon 66, nylon 610, nylon 10 and nylon 12.
3. The method for preparing a nylon film having puncture resistance and high surface wetting tension as claimed in claim 1, characterized in that: The following steps are involved: Step 1, preparing modified nylon particles; step 2, stretching nylon film; step 3, preparing nylon film; In step 1, nylon particles, a cross-linking-wetting dual-effect modifier, an auxiliary cross-linking agent, tetradimethylvinylsiloxysilane, a photoinitiator, 2-hydroxy-2-methylpropiophenone and nano-silica are added to a twin-screw extruder in proportion for blending and granulation, and the three-zone temperatures are 140° C., 180° C. and 170° C. to obtain modified nylon particles; In step 2, the modified nylon particles are added into a casting machine for extrusion casting, and the cast sheet is synchronously biaxially stretched to obtain a biaxially stretched nylon film, the stretching temperature is 140-170° C., the transverse stretching ratio is 1.6-1.9, and the longitudinal stretching ratio is 1.8-2.8; In step three, the biaxially stretched nylon film is irradiated with low-power ultraviolet light with a wavelength range of 350 to 400 nm, a power of 10 to 25 W, and an irradiation time of 10 to 30 seconds to obtain a nylon film with puncture resistance and high surface wetting tension.
4. The use of a nylon film having puncture resistance and high surface wetting tension as claimed in claim 1, characterized in that: A composite polyurethane adhesive with a thickness of 5 to 20 μm is evenly coated on the aluminum foil surface of the aluminum foil / polypropylene film, and then a nylon film with puncture resistance and high surface wetting tension is pressed onto the adhesive, and an aluminum-plastic composite film for lithium-ion batteries is obtained after curing.