Silicon dioxide@intrinsic self-polymerizing composite material and its preparation method and application

Through the combination of silicon oxide and intrinsic self-polymerizing materials, self-healing is achieved using reversible non-covalent hydrogen bonds, which solves the problems of volume change and structural instability of silicon-based materials in lithium-ion batteries, and improves the cycle stability of the material. reliability and service life, and realizes the resource reuse of silicon oxide waste, improving the performance of lithium-ion batteries.

CN118054003BActive Publication Date: 2024-10-01KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410260870.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-07
Publication Date
2024-10-01
Estimated Expiration
2044-03-07

AI Technical Summary

Technical Problem

The volume changes of silicon-based materials in existing lithium-ion batteries, the continued growth of the SEI film, and the low lithium ion diffusivity lead to unstable material structures and reduced service life, and the recycling and reuse of silicon oxide waste is difficult to achieve.

Method used

Silicon oxide is used to composite with intrinsic self-polymerizing materials, and the self-polymerization of the material is realized through reversible non-covalent hydrogen bonding to form silicon oxide@intrinsic self-polymerizing composite materials, and ester materials are used to interact with methyl methacrylate. The reversible dynamic bonds of the self-healing material are reorganized at the damaged site to maintain the stability of the material structure.

Benefits of technology

It improves the cycle stability and service life of silica@intrinsic self-polymerizing composite materials, realizes the resource reuse of silica waste, reduces electrode side reactions, and significantly improves the performance and efficiency of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118054003B_ABST
    Figure CN118054003B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of self-polymerizing negative electrode materials for lithium-ion batteries, and particularly relates to silicon dioxide @ intrinsic self-polymerizing composite materials and preparation methods and applications thereof. The present invention uses ester materials and methyl methacrylate as raw materials to perform cross-linking polymerization to obtain intrinsic self-polymerizing materials, and simultaneously uses the intrinsic self-polymerizing materials and silicon dioxide materials for composite, and realizes self-polymerization through reversible non-covalent hydrogen bonds of the self-polymerizing materials, so that after the silicon dioxide undergoes volume changes during the cycle, the structural stability of the silicon dioxide @ intrinsic self-polymerizing composite materials can be maintained, thereby improving the cycle stability and service life of the composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion battery self-polymerization negative electrode materials, and in particular relates to silicon dioxide @ intrinsic self-polymerization composite materials and a preparation method and application thereof. Background Art

[0002] As the scale of the new energy vehicle market continues to expand, the demand for high specific energy and long life lithium-ion batteries is increasing year by year. Commercial graphite anode materials have a low theoretical specific capacity (372 mAhg -1 ) can no longer meet the current demand for lithium-ion batteries. Silicon has abundant reserves and a high theoretical specific capacity (4200mAhg -1 ) advantages, making it one of the excellent negative electrode materials.

[0003] Silicon and silicon oxide, due to their advantages such as high lithium storage capacity, high lithium insertion potential and abundant natural reserves, can meet the growing demand for energy storage in portable electronic devices such as pacemakers, biomedical micro-nano motor power supplies, as well as various technologies in electric vehicles and energy storage systems. In particular, silicon-based negative electrode materials mainly composed of silicon oxide have become one of the key negative electrode materials for the new generation of lithium-ion batteries.

[0004] At present, the production of silicon oxide is mainly based on chemical vapor deposition. However, in the actual production process, a large amount of silicon oxide fine powder particles will be produced. These particles have high reactivity, poor conductivity, and low compaction density. They are not suitable for direct use as negative electrode materials for lithium-ion batteries and are a waste of resources. Therefore, facing the frontier hotspot of recycling and reuse of silicon oxide waste, it is of great significance to further process silicon oxide fine powder waste materials. However, silicon oxide as a negative electrode has the disadvantages of severe volume change, continuous growth of SEI film, and low lithium ion diffusion rate, which hinders the large-scale commercial application of silicon oxide.

[0005] In the prior art, when dealing with the volume change of silicon-based materials as negative electrode materials, the continuous growth of SEI film, and the low lithium ion diffusion rate, silicon-based materials are often compounded with other materials to overcome the above technical defects. Mai et al. used high-energy ball milling to grind micronized SiOx with m-phenylenediamine and hexamethylenetetramine in a glove box, then put them in an autoclave for curing and annealing to obtain nitrogen-doped carbon-coated SiOx (SiOx@NC), which has a capacity of 774 mAhg -1The reversible specific capacity of the battery can be achieved, and the capacity retention rate after 500 cycles is 112%. This method that does not require solvents or combustible gases is also applicable to other alloy conversion negative electrodes. However, even if a composite material is obtained, and space is provided in the composite material for the volume change of the silicon-based material, the volume change of the silicon-based material during the cycle still has a great impact on the structure and performance of the entire composite material, which in turn affects the overall structural stability of the composite material and reduces the service life of the composite material. Summary of the invention

[0006] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a silicon oxide @ intrinsic self-polymerizing composite material and a preparation method and application thereof. The present invention uses an intrinsic self-polymerizing material and a silicon oxide material for compounding, and realizes its self-polymerization through the reversible non-covalent hydrogen bonds of the self-polymerizing material, so that after the silicon oxide undergoes volume changes during the cycle, the structural stability of the silicon oxide @ intrinsic self-polymerizing composite material can still be maintained, thereby improving the cycle stability and service life of the composite material.

[0007] In order to achieve the above purpose, the technical solution adopted in this application is:

[0008] A method for preparing a silicon dioxide@intrinsic self-polymerizing composite material comprises the following steps:

[0009] Silicon dioxide, ester materials and methyl methacrylate are mixed, and then an initiator is added to realize cross-linking polymerization of the ester materials and methyl methacrylate. The cross-linking polymerization process is that the reversible non-covalent hydrogen bonds of methyl methacrylate and the polar covalent polyurethane polymers containing ester materials are cross-linked by esterification to construct a network structure. The chemical bonds of the self-polymerization are reversible non-covalent hydrogen bonds. When the self-healing material is damaged, the reversible dynamic bonds will break before the traditional covalent bonds due to their weaker interactions. When the damage area is not large, these reversible dynamic bonds are reorganized at the fracture to generate new bonds to repair the damage, thereby obtaining silicon dioxide @ intrinsic self-polymerization material;

[0010] After the silicon dioxide @ intrinsic self-polymerizing material is dried to constant weight, it is sintered at low temperature in an inert atmosphere to ensure the internal dryness of the particles and improve the stability of the internal structure, thereby obtaining a silicon dioxide @ intrinsic self-polymerizing composite material.

[0011] Preferably, the particle size of silicon oxide is 0.4-3 μm, and the morphology of silicon oxide can be selected from flake, dendrite, spherical, pebble, irregular shape, etc. The silicon oxide raw material of the present invention is the waste material left after preparing silicon oxide by chemical vapor deposition method, so as to realize the reprocessing and utilization of waste material; research shows that in the electrochemical cycle process, the structural stability of silicon is closely related to its size, and the crystalline Si particles with a particle size less than 150nm will not break during lithiation, but the development cost of nano silicon is too high. Compared with the nanoscale, the micrometer-scale silicon material has a higher tap density and can achieve a higher volume capacity under the same mass load; in addition, the lower specific surface area of ​​the particles can significantly reduce harmful side reactions, thereby improving the initial coulomb efficiency of the electrode. Under the condition of the same electrode thickness, the electrode composed of micrometer-scale particles has a higher surface capacity.

[0012] Preferably, the ester material is selected from formate materials, acetate materials or acrylate materials, and its weight average molecular weight is 80,000-800,000. Formate materials include ethyl benzoate, isopentyl formate, etc., acetate materials include ethyl acetate, benzyl acetate, etc., and propionate materials include n-butyl acrylate, n-pentyl acrylate.

[0013] Preferably, the initiator is selected from an organic peroxide initiator, a redox initiator system or an azo initiator, the organic peroxide initiator is selected from cumene peroxide or diisopropyl percarbonate; the redox initiator system is selected from benzoyl oxide / N,N , -dimethylaniline, ammonium persulfate / sodium bisulfite; the azo initiator is selected from azobisisobutyronitrile; under the action of the initiator, the monomer molecules will be excited to become free radicals or ions in the reaction, thereby starting the polymerization reaction. The reason why the initiator can initiate the polymerization reaction is that it can weaken the bond strength between monomers, promote the stability of the polymerization product and expand the reaction space. The purpose of adding the initiator is to start the reaction and accelerate the reaction rate.

[0014] Preferably, the mass ratio of the initiator, the ester material and methyl methacrylate is 1:200-500:200-500, further 1:500:200, and the mass ratio of silicon oxide to the intrinsic self-polymerizing material is 1:5-5:1, preferably 1:2-2:1.

[0015] Preferably, the cross-linking polymerization condition is: stirring at room temperature for 12-24 hours.

[0016] Preferably, the low-temperature sintering conditions are: sintering at 180-200°C for 3-6h. Too high a temperature or too long a time will destroy the integrity of the internal structure, while too low a temperature or too short a time will result in incomplete internal chemical reactions, affecting the stability of the material at different temperatures.

[0017] The present invention also protects the silicon dioxide @ intrinsic self-polymerizing composite material obtained by the above-mentioned preparation method. The silicon in the silicon dioxide @ intrinsic self-polymerizing composite material can be amorphous or crystalline, or the above-mentioned two forms can coexist. The particle size of the composite material is 800nm-10μm. The silicon dioxide @ intrinsic self-polymerizing composite material has a high degree of compositeness and will not be too large to cause structural instability.

[0018] The present invention also protects the application of silicon monoxide @ intrinsic self-polymerization composite material in the preparation of negative electrode materials for lithium ion batteries.

[0019] Preferably, the application method is: dispersing the silicon dioxide @ intrinsic self-polymerization composite material, the conductive agent and the adhesive in acetone to obtain a slurry, coating the slurry on a current collector, and drying to obtain a negative electrode material for a lithium ion battery;

[0020] The mass ratio of silicon dioxide@intrinsic self-polymerizing composite material to conductive agent and adhesive is 8:1:1;

[0021] The conductive agent is selected from conductive carbon black, carbon nanotubes or graphene; the binder is selected from polyvinylidene fluoride or carboxymethyl cellulose; and the solvent is selected from N-methylpyrrolidone or deionized water.

[0022] Compared with the prior art, the beneficial effects of this application are:

[0023] 1. Intrinsic self-polymerizing materials are polymerized by incorporating reversible covalent bonds or non-covalent bonds into the polymer system. When the self-healing material is damaged, the reversible dynamic bonds will break before the traditional covalent bonds due to their weaker interactions. Under certain conditions, these reversible dynamic bonds will reorganize at the break to generate new bonds to repair the damage. This process does not require any additional polymerizing agents, and in principle can infinitely restore its chemical or physical properties, and eliminates the cumbersome polymerizing agent encapsulation process of external self-polymerizing materials.

[0024] 2. The present invention adopts ester materials, methyl methacrylate and initiators to prepare self-polymerizing materials. There is a thin oxide layer containing hydroxyl groups on the surface of natural silicon. Therefore, polymers rich in hydroxyl groups and carboxyl groups usually have a higher bonding strength to silicon. The self-polymerizing material also contains a part of hydroxyl groups and carboxyl groups. Therefore, it can form a bond with the hydroxyl oxide layer. The formed bond has a certain bonding strength, which promotes the bonding between the two.

[0025] In addition, the silicon oxide powder of the present application is obtained from waste materials of industrial production of nano silicon oxide and battery recycling process, and the silicon oxide waste materials in the actual production process are reprocessed and reused, thereby achieving full utilization of resources.

[0026] 3. Compared with the existing technology, the preparation method provided by the present invention is simple, low in cost, highly practical and can be prepared on a large scale. The intrinsic self-polymerizing material can withstand the volume expansion of the active material and inhibit the formation of large cracks due to its excellent tensile strength (about 50MPa) and strong interaction with the active material. The reversible dynamic bond is easily broken to dissipate energy when subjected to external strain, which makes the electrode more resistant to strain and volume expansion. On the other hand, the self-healing material can be used as an electrolyte or protective shell of the battery. Once the equipment is damaged, it only needs to re-contact the fracture surface. After the fracture, it will begin to polymerize inward at the edge of the crack until it is fully contacted to restore the mechanical and electrochemical properties. It can be seen that the self-polymerization function has broad application prospects in the field of electronics. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a SEM electron microscope image of the silicon dioxide @ intrinsic self-polymerization composite material obtained in Example 1;

[0028] Figure 2 This is a SEM electron microscope image of the silicon dioxide @ intrinsic self-polymerization composite material obtained in Example 2;

[0029] Figure 3 The cycle performance diagrams of the lithium ion battery prepared by using the silicon dioxide @ intrinsic self-polymerization composite material of Example 1 after 1 cycle, 3 cycles and 100 cycles;

[0030] Figure 4 The XRD diagrams of the lithium ion battery prepared by using the silicon dioxide @ intrinsic self-polymerization composite material of Example 1 after 1 cycle and 100 cycles. DETAILED DESCRIPTION

[0031] The specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work belong to the scope of protection of the present invention. The raw materials used in the present invention without indicating the manufacturer are all conventional products that can be purchased commercially.

[0032] The present invention adopts ester materials, methyl methacrylate and initiators to prepare self-polymerizing materials, and prepares composite materials with silicon oxide during the self-polymerization process. The theoretical specific capacity of silicon oxide is as high as 2043mAh / g. At the same time, silicon oxide has a lithium insertion platform close to that of graphite, making it one of the most promising next-generation high-capacity negative electrode materials. During the first lithium insertion process, silicon dioxide reacts with lithium to generate lithium oxide and lithium silicate. On the one hand, lithium oxide and lithium silicate can buffer the expansion effect of silicon-lithium alloy (about ≈118%), and on the other hand, they inhibit silicon agglomeration to a certain extent, but the expansion problem is still very serious. Taking this technical problem into consideration, the present application uses a self-polymerizing material and silicon dioxide for compounding. The reversible dynamic bonds of the self-polymerizing material will break before the traditional covalent bonds due to their weaker interactions. Under certain conditions, these reversible dynamic bonds will rearrange at the fracture to generate new bonds to repair the damage. Therefore, the purpose of structural recovery is achieved without the need for any additional polymerizing agent, and the secondary utilization of silicon dioxide waste is achieved, thereby obtaining a new material with high cyclic stability. The silicon dioxide @ intrinsic self-polymerizing composite material has an excellent service life after being used in lithium-ion batteries.

[0033] In addition, the present invention uses micron-sized silicon dioxide as a raw material and directly compounds it with a self-polymerizing material, thereby reducing interface side reactions while maintaining the specific surface area of ​​silicon dioxide.

[0034] It should be understood that the terms described in the present invention are only for describing specific embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope. The following uses examples and comparative examples to further compare and study the technical solutions of the present application, as shown below:

[0035] Example 1

[0036] A method for preparing a silicon dioxide@intrinsic self-polymerizing composite material comprises the following steps:

[0037] S1. Silicon dioxide with an average particle size of 3 μm, ester materials n-pentyl acrylate and methyl methacrylate are mixed, and an initiator azobisisobutyronitrile is added. Toluene is used as a solvent, and the mixture is stirred and polymerized at room temperature for 12 hours, and then ultrasonicated at 40 kHz for 2 minutes. The purpose of ultrasonication is to prevent adhesion and agglomeration caused by too long stirring time, so as to obtain silicon dioxide @ intrinsic self-polymerizing material;

[0038] The mass ratio of silicon oxide, ester materials n-pentyl acrylate, methyl methacrylate, and azobisisobutyronitrile is 100:50:20:0.1;

[0039] S2. After drying the silicon dioxide @ intrinsic self-polymerizing material, sinter it at 200° C. for 3 h in an argon atmosphere at a heating rate of 1° C. / min to obtain a spherical silicon dioxide @ intrinsic self-polymerizing composite material.

[0040] Example 2

[0041] A method for preparing a silicon dioxide@intrinsic self-polymerizing composite material comprises the following steps:

[0042] S1. Silicon dioxide with an average particle size of 2 μm, ester materials benzyl acetate and methyl methacrylate are mixed, and an initiator cumene peroxide is added. Tetrahydrofuran is used as a solvent, and the mixture is stirred and polymerized at room temperature for 12 hours, and then ultrasonicated at 40 kHz for 3 minutes. The purpose of ultrasonication is to prevent adhesion and agglomeration caused by too long stirring time, so as to obtain silicon dioxide @ intrinsic self-polymerizing material;

[0043] The mass ratio of silicon oxide, ester materials benzyl acetate, methyl methacrylate, and cumene peroxide is 100:50:30:0.1;

[0044] S2. After drying the silicon dioxide @ intrinsic self-polymerizing material, sinter it at 190° C. for 4 h in an argon atmosphere at a heating rate of 1° C. / min to obtain a spherical silicon dioxide @ intrinsic self-polymerizing composite material.

[0045] Example 3

[0046] A method for preparing a silicon dioxide@intrinsic self-polymerizing composite material comprises the following steps:

[0047] S1. Silicon dioxide with an average particle size of 1 μm, ester materials isoamyl formate and methyl methacrylate are mixed, and an initiator diisopropyl percarbonate is added. Tetrahydrofuran is used as a solvent, and the mixture is polymerized under magnetic stirring for 24 hours at room temperature, and then ultrasonicated at 20 kHz for 4 minutes. The purpose of ultrasonication is to prevent adhesion and agglomeration caused by too long stirring time, so as to obtain silicon dioxide @ intrinsic self-polymerizing material;

[0048] The mass ratio of silicon oxide, ester materials isopentyl formate, methyl methacrylate, and diisopropyl percarbonate is 100:30:50:0.1;

[0049] S2. After drying the silicon dioxide @ intrinsic self-polymerizing material, sinter it at 180° C. for 5 h in an argon atmosphere at a heating rate of 1° C. / min to obtain a spherical silicon dioxide @ intrinsic self-polymerizing composite material.

[0050] Example 4

[0051] A method for preparing a silicon dioxide@intrinsic self-polymerizing composite material comprises the following steps:

[0052] S1. Silicon oxide with an average particle size of 500 nm, ester materials n-butyl acrylate and methyl methacrylate are mixed, and an initiator cumene peroxide is added. Tetrahydrofuran is used as a solvent, and the mixture is polymerized under magnetic stirring for 18 hours at room temperature, and ultrasonicated at 20 kHz for 5 minutes. The purpose of ultrasonication is to prevent adhesion and agglomeration caused by too long stirring time, so as to obtain silicon oxide @ intrinsic self-polymerizing material;

[0053] The mass ratio of silicon oxide, ester materials n-butyl acrylate, methyl methacrylate, and cumene peroxide is 100:20:50:0.1;

[0054] S2. After drying the silicon dioxide @ intrinsic self-polymerizing material, sinter it at 180° C. for 6 h in an argon atmosphere at a heating rate of 1° C. / min to obtain a spherical silicon dioxide @ intrinsic self-polymerizing composite material.

[0055] Example 5

[0056] A method for preparing a silicon dioxide@intrinsic self-polymerizing composite material comprises the following steps:

[0057] S1. Silicon dioxide with an average particle size of 500 nm, ester materials n-butyl acrylate and methyl methacrylate are mixed, and an initiator cumene peroxide is added. Tetrahydrofuran is used as a solvent, and the mixture is polymerized under magnetic stirring for 20 hours at room temperature, and ultrasonicated at 20 kHz for 5 minutes. The purpose of ultrasonication is to prevent adhesion and agglomeration caused by too long stirring time, so as to obtain silicon dioxide @ intrinsic self-polymerizing material;

[0058] The mass ratio of silicon oxide, ester materials n-butyl acrylate, methyl methacrylate, and cumene peroxide is 100:250:250:0.1;

[0059] S2. After drying the silicon dioxide @ intrinsic self-polymerizing material, sinter it at 190° C. for 5 h in an argon atmosphere at a heating rate of 1° C. / min to obtain a spherical silicon dioxide @ intrinsic self-polymerizing composite material.

[0060] Example 6

[0061] A method for preparing a silicon dioxide@intrinsic self-polymerizing composite material comprises the following steps:

[0062] S1. Silicon oxide with an average particle size of 400 nm, ester materials n-butyl acrylate and methyl methacrylate are mixed, and an initiator cumene peroxide is added. Tetrahydrofuran is used as a solvent, and the mixture is polymerized under magnetic stirring for 15 hours at room temperature, and ultrasonicated at 20 kHz for 5 minutes. The purpose of ultrasonication is to prevent adhesion and agglomeration caused by too long stirring time, so as to obtain silicon oxide @ intrinsic self-polymerizing material;

[0063] The mass ratio of silicon oxide, ester materials n-butyl acrylate, methyl methacrylate, and cumene peroxide is 100:10:10:0.1;

[0064] S2. After drying the silicon dioxide @ intrinsic self-polymerizing material, sinter it at 200° C. for 4 h in an argon atmosphere at a heating rate of 1° C. / min to obtain a spherical silicon dioxide @ intrinsic self-polymerizing composite material.

[0065] Comparative Example 1

[0066] The preparation steps of this comparative example are the same as those of Example 1, except that the intrinsic self-polymerizing material is not used to compound with silicon oxide to obtain a bulk silicon oxide negative electrode material, which specifically includes the following steps:

[0067] S1. Dissolve silicon dioxide with an average particle size of 3 μm in ultrapure water, stir magnetically for 12 h at room temperature, and ultrasonicate at 20 kHz for 40 min to obtain a precursor;

[0068] S2. After drying the precursor in an air atmosphere, sinter it in an argon atmosphere at 200° C. for 3 h with a heating rate of 1° C. / min to obtain a bulk silicon dioxide negative electrode material.

[0069] Comparative Example 2

[0070] The preparation steps of this comparative example are the same as those of Example 1, except that a non-intrinsic self-polymerizing material phenolic resin is used to compound with silicon dioxide to obtain a silicon dioxide@phenolic resin composite material, which specifically includes the following steps:

[0071] S1, dissolving silicon dioxide with an average particle size of 3 μm and phenolic resin in ultrapure water, magnetically stirring at room temperature for 12 h, and then ultrasonicating at 20 kHz for 40 min to obtain a precursor;

[0072] S2. After drying the precursor in an air atmosphere, sintering it in an argon atmosphere at 200° C. for 3 h at a heating rate of 1° C. / min to obtain a silicon dioxide@phenolic resin composite material.

[0073] Examples 1-6 of the present invention all prepared silicon dioxide @ intrinsic self-polymerizing composite materials with excellent electrochemical cycle performance, and the effects were similar. The silicon dioxide @ intrinsic self-polymerizing composite materials of Examples 1-4 were taken as examples and compared with Comparative Examples 1-2. The specific research methods and results are as follows:

[0074] 1. Morphology characterization: The particle size and particle size distribution of the spherical silicon dioxide @ intrinsic self-polymerization composite materials obtained in Examples 1-4 were detected by TESCAN VEGA3 scanning electron microscope. The results showed that the particle size distribution of the spherical silicon dioxide @ intrinsic self-polymerization composite materials was relatively uniform. The particle size of the composite material obtained in Example 1 was between 400nm and 10μm (e.g. Figure 1 The particle size of the composite material obtained in Example 2 is between 4 and 10 μm (as shown in Figure 2 As shown), the particle size of the composite material obtained in Example 3 is between 6-12 μm, and the particle size of the composite material obtained in Example 4 is between 6-15 μm.

[0075] 2. Battery production: The spherical silicon oxide @ intrinsic self-polymerizing composite material prepared in Examples 1-4, conductive carbon black SuperP, CMC (carboxymethyl cellulose, binder) and SBR (styrene-butadiene rubber, binder) were weighed in a mass ratio of 70:15:5:10, and then dispersed in deionized water, mechanically mixed until the mixture was viscous and gelatinous to obtain a slurry, and the slurry was evenly coated on the surface of the current collector copper foil by an automatic coating machine with a thickness of 200 μm. After that, the pole piece coated with the slurry was placed in a vacuum drying oven at 60°C and dried for 8 hours, and cut into circular pole pieces with a diameter of 14 mm under a manual punching machine, and then weighed for use;

[0076] Assemble the button battery in a glove box filled with argon gas, and assemble the CR2025 button battery. Use metal lithium sheet as the counter electrode, Whatman GF / C as the separator, LX-025 as the electrolyte, add the positive electrode shell, negative electrode shell, gasket and spring, and seal it with a button battery sealing machine. Perform the charge and discharge test. The test procedure is 300mA / g, and the charge and discharge voltage range is 0.01V-1.5V. The cycle curve and coulomb efficiency are shown in Table 1.

[0077] The silicon dioxide @ intrinsic self-polymerization composite material of Example 1 has a first charge and discharge cycle efficiency of 60.00%, an initial charge capacity of 1566.76 mAh / g, and after 100 cycles, a charge specific capacity of 1096.73 mAh / g, and a capacity retention rate of 42% within 100 cycles.

[0078] Table 1 Cyclic performance results of silicon dioxide@intrinsic self-polymerizing composite materials of Examples 1-4 and Comparative Example 1

[0079]

[0080]

[0081] It can be clearly seen from the results in Table 1 that the cycle performance of the silicon dioxide negative electrode material prepared in the embodiment is significantly better than the cycle performance of the control example without adding intrinsic self-polymerizing material. This shows that the secondary granulation modification of micron-sized silicon dioxide in the present invention greatly optimizes the cycle performance of silicon dioxide, thereby meeting the social demand for solving the waste of micron-sized silicon dioxide.

[0082] Table 2 Material cycle performance results of Example 1 and Comparative Examples 1-2

[0083] serial number First coulombic efficiency Capacity retention rate after 3 cycles 200 cycles capacity retention rate Example 1 68% 44% 38% Comparative Example 1 61% 40% 5% Comparative Example 2 64% 42% 16%

[0084] Table 2 is a comparative analysis of the capacity retention rates of Example 1, Comparative Example 1, and Comparative Example 2. It can be analyzed that the capacity loss rates of the three groups of experiments in the first three cycles are similar, which is a capacity loss phenomenon in the normal silicon oxide cycle process. In the subsequent 200 cycles, the intrinsic self-polymerization material maintained a high cycle performance, while the capacity of the unused group and the group using other materials decreased rapidly after 200 cycles, proving that the material was damaged during use, resulting in irreversible loss of performance.

[0085] like Figure 3 The electrochemical performance of the material prepared in Example 1 is shown, and the data of 1 cycle, 3 cycles, and 100 cycles are taken respectively. The difference between the first cycle and the third cycle is the loss during the battery activation process, which is a normal phenomenon. The capacity loss rate of the subsequent 3-100 cycles is extremely low. It can be basically analyzed that the self-polymer material continuously heals itself during the battery cycle to ensure the structural integrity of the material. From this, it can be analyzed that the self-polymer material has a significant effect in ensuring cycle stability.

[0086] Figure 4 The XRD graph shows that there is no obvious change before and after 100 cycles, proving that no other side reactions occur during the use of the material to consume the electrode material, ensuring the stability of the cycle process.

[0087] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a silicon oxide @ intrinsic self-polymerizing composite material, characterized in that: The steps include: Mixing silicon dioxide, an ester material and methyl methacrylate, and then adding an initiator to achieve cross-linking polymerization of the ester material and methyl methacrylate to obtain silicon dioxide @ intrinsic self-polymerizing material; After drying the silicon dioxide @ intrinsic self-polymerizing material to a constant weight, sintering at a low temperature in an inert atmosphere to obtain a silicon dioxide @ intrinsic self-polymerizing composite material; The ester material is selected from n-butyl acrylate, isoamyl formate, benzyl acetate, and n-amyl acrylate; The mass ratio of the initiator, the ester material and the methyl methacrylate is 1:200-500:200-500.

2. The method for preparing the silicon dioxide intrinsic self-polymerization composite material according to claim 1, characterized in that: The initiator is selected from an organic peroxide initiator, a redox initiator system or an azo initiator.

3. The method for preparing the silicon dioxide intrinsic self-polymerization composite material according to claim 1, characterized in that: The mass ratio of silicon monoxide to the intrinsic self-polymerizing material is 1:5-5:

1.

4. The method for preparing the silicon 2 Oxide @ intrinsic self-polymerization composite material according to claim 1, characterized in that: The cross-linking polymerization conditions are: stirring at room temperature for 12-24 hours.

5. The method for preparing the silicon dioxide intrinsic self-polymerization composite material according to claim 1, characterized in that: The low-temperature sintering conditions are: sintering at 180-200° C. for 3-6 hours.

6. The method for preparing the silicon dioxide intrinsic self-polymerization composite material according to claim 1, characterized in that: The particle size of silicon monoxide is 0.4-3 μm.

7. A silicon dioxide intrinsic self-polymerizing composite material obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The silicon in the silicon oxide@intrinsic self-polymerization composite material mainly exists in an amorphous form, and the particle size of the composite material is 800nm-10μm.

8. Use of the silicon dioxide@intrinsic self-polymerization composite material according to claim 7 in preparing a negative electrode material for a lithium-ion battery.

9. The use according to claim 8, characterized in that The application method is: The silicon dioxide @ intrinsic self-polymerization composite material, a conductive agent and an adhesive are dispersed in acetone to obtain a slurry, and the slurry is coated on a current collector and dried to obtain a lithium ion battery negative electrode material.