A torsion-resistant aluminum alloy wind power cable and a manufacturing method thereof

By adopting different aluminum alloy formulas and multiple aging treatment methods, the tensile strength and toughness of aluminum alloy wind energy cables are improved, and the problem of easily breaking conductors during torsion is solved, and the high-cycle torsional capacity and cost reduction of cables is achieved. Copper core twisted cables have been used to reduce the procurement cost of wind turbines.

CN118073018BActive Publication Date: 2024-11-12C KINGDOM CABLE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410267198.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-08
Publication Date
2024-11-12
Estimated Expiration
2044-03-08

AI Technical Summary

Technical Problem

When existing aluminum alloy wind energy cables frequently twist in complex environments such as high temperature, high humidity, salt spray, etc., the outer layer of the conductor is prone to break and cannot pass the 10,000-cycle room temperature torsion test, resulting in the use pattern of copper core torsion cables and increasing wind power. The procurement cost of the unit.

Method used

Three different aluminum alloy formulas are used to make the outermost layer, middle layer and central layer strands of the cable conductor, and the tensile strength, toughness and creep resistance of the conductor are improved through multiple aging treatments to ensure that the cable is not easy to twist during the twisting process. fracture.

Benefits of technology

By improving the formulation and manufacturing process of aluminum alloy conductors, the torsion resistance of aluminum alloy cables is improved, and the 15,000-cycle torsion test is able to pass the normal temperature torsion test, reducing material costs, and replacing copper core torsion cables, reducing wind turbine cable procurement cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118073018B_ABST
    Figure CN118073018B_ABST
Patent Text Reader

Abstract

The invention discloses a torsion-resistant aluminum alloy wind power cable and a manufacturing method thereof. The cable comprises an aluminum alloy conductor, which comprises an outermost aluminum alloy strand, an intermediate aluminum alloy strand and a central aluminum alloy strand; the cable conductor is made of different aluminum alloy formulas for the outermost layer, the intermediate layer and the central layer, and the aluminum alloy formula of the outermost aluminum alloy strand comprises the following components by mass percentage: Si 0.4%-0.6%, Fe 0.1%-0.3%, Cu 0.02%-0.05%, Mn 0.01%-0.02%, Mg0.35%-0.5%, Cr 0.01%-0.02%, Zn≤0.10%, B 0.01%-0.05%, Li 0.001%-0.005%, Zr 0.003%-0.01%, Sn 0.001%-0.005%, Sc 0.016%-0.02%, each impurity element ≤0.03%, total impurity element ≤0.10%, and the rest is aluminum. The cable conductor of the present invention has been subjected to four aging treatments, and the cable using the conductor can pass 11,000 cycles or 15,000 cycles of normal temperature torsion test, and has lower cost than copper core twist cable, which is in line with the development trend of wind power energy parity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cables, and in particular relates to a torsion-resistant aluminum alloy wind power cable and a manufacturing method thereof. Background Art

[0002] Torsion-resistant wind power cables are widely installed in complex environments such as high temperature, high humidity, salt spray, and large temperature differences. The cables are frequently twisted during operation. Therefore, the cables are required to be resistant to high and low temperatures, oil, salt spray, UV, and moisture, and to ensure that the cables can pass more than 10,000 cycles of torsion tests at room temperature (clockwise twisting 1440° to restore to the initial state, and then counterclockwise twisting the same angle to restore to the initial state, which is one cycle) and 2,000 or 5,000 cycles of low-temperature torsion tests. With the advent of the era of large-scale wind power parity, it has become a trend for aluminum alloy cables in the fixed section of the tower to replace copper core cables. However, the twisted cable section that needs to be twisted is still a copper core twisted cable. At present, the aluminum alloy core conductors used in the wind power cable industry generally use 8030 aluminum alloy, and in the existing manufacturing process, only the aluminum alloy conductor rods and conductor monofilaments are generally annealed, and the conductor strands and the conductors after re-twisting are not aged. Therefore, it cannot be ensured that the cable can pass the 10,000 cycle room temperature torsion test. Therefore, it is very necessary to solve the bottleneck problem that the current aluminum alloy wind power cable cannot pass the 10,000-cycle room temperature torsion test, overturn the pattern of using copper core twisted cables in the torsion section of wind turbines, lead the market, and reduce the procurement cost of wind turbine cables. Summary of the invention

[0003] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a torsion-resistant aluminum alloy wind power cable and a manufacturing method thereof, thereby improving the torsion resistance of the aluminum alloy cable by improving the cable aluminum alloy conductor formula and the manufacturing method thereof.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] In the early stage of the research, the inventor conducted a torsion test on the cable using 8030 aluminum alloy as the conductor in the prior art and found that broken wires mainly occurred in the outermost strands. Therefore, in order to solve the problem that the outer layer of the cable conductor is easy to break when twisted, the present invention improves the formula of the aluminum alloy conductor, and adopts two or three aluminum alloy formulas to respectively make the outermost strands, middle strands and center strands of the cable conductor. Among them, the outermost strands of the conductor are made of aluminum alloy with high tensile strength, high toughness, creep resistance, heat resistance and corrosion resistance, the middle layer strands are made of creep-resistant aluminum alloy wire with adjusted formula, and the center layer strands are preferably made of creep-resistant and high tensile aluminum alloy wire. Specifically:

[0006] The invention provides a torsion-resistant aluminum alloy wind power cable, comprising an aluminum alloy conductor, wherein the aluminum alloy conductor comprises an outermost aluminum alloy strand, an intermediate aluminum alloy strand and a center aluminum alloy strand; the aluminum alloy formula of the outermost aluminum alloy strand comprises the following components by mass percentage: Si 0.4%-0.6%, Fe 0.1%-0.3%, Cu 0.02%-0.05%, Mn 0.01%-0.02%, Mg 0.35%-0.5%, Cr 0.01%-0.02%, Zn≤0.10%, B 0.01%-0.05%, Li 0.001%-0.005%, Zr 0.003%-0.01%, Sn 0.001%-0.005%, Sc 0.016%-0.02%, each impurity element is ≤0.03%, the total amount of impurity elements is ≤0.10%, and the rest is aluminum.

[0007] Preferably, the aluminum alloy formula of the intermediate layer aluminum alloy strand includes the following components by mass percentage: Si 0.05%-0.1%, Fe 0.3%-0.4%, Cu 0.10%-0.20%, Mg 0.001%-0.005%, Zn 0.005%-0.01%, B 0.001%-0.01%, Li 0.001%-0.005%, Sc 0.0015%-0.017%, each impurity element ≤0.03%, the total amount of impurity elements ≤0.10%, and the rest is aluminum.

[0008] Preferably, the aluminum alloy formula of the center layer aluminum alloy strand is:

[0009] The following components are included by mass percentage: Si 0.05%-0.1%, Fe 0.3%-0.4%, Cu0.10%-0.20%, Mg 0.001%-0.005%, Zn 0.005%-0.01%, B 0.001%-0.01%, Li0.001%-0.005%, Sc 0.0015%-0.017%, each impurity element ≤0.03%, the total amount of impurity elements ≤0.10%, and the rest is aluminum;

[0010] Or includes the following components by mass percentage: Si 0.6%-0.7%, Fe 0.2%-0.3%, Cu0.01%-0.015%, Mn 0.01%-0.02%, Mg 0.35%-0.5%, Cr 0.01%-0.02%, Zn≤0.10%, B0.01%-0.05%, Li 0.001%-0.005%, Sn 0.001%-0.005%, Sc 0.016%-0.020%, each impurity element ≤0.03%, the total amount of impurity elements ≤0.10%, and the rest is aluminum.

[0011] The present invention also provides a method for manufacturing the torsion-resistant aluminum alloy wind power cable, comprising the following steps:

[0012] 1) Manufacturing aluminum alloy rods: the outermost aluminum alloy rod is manufactured according to the aluminum alloy formula of the outermost aluminum alloy strands; the middle layer aluminum alloy rod is manufactured according to the aluminum alloy formula of the middle layer aluminum alloy strands; the center layer aluminum alloy rod is manufactured according to the aluminum alloy formula of the center layer aluminum alloy strands;

[0013] 2) Aging treatment of aluminum alloy rods: Aging treatment is performed on the outermost aluminum alloy rod, the middle layer aluminum alloy rod, and the center layer aluminum alloy rod respectively;

[0014] 3) Aluminum alloy monofilament drawing: the outermost aluminum alloy rod, the middle aluminum alloy rod, and the center aluminum alloy rod after aging treatment are drawn into the outermost aluminum alloy monofilament, the middle aluminum alloy monofilament, and the center aluminum alloy monofilament respectively;

[0015] 4) Aging treatment of aluminum alloy monofilaments: Aging treatment is performed on the outermost aluminum alloy monofilament, the middle aluminum alloy monofilament, and the center aluminum alloy monofilament respectively;

[0016] 5) Aluminum alloy monofilament bundle twisting: The outermost aluminum alloy monofilament, the middle aluminum alloy monofilament and the center aluminum alloy monofilament after aging treatment are bundled into strands on a bundle twisting machine to obtain the outermost aluminum alloy strand, the middle aluminum alloy strand and the center aluminum alloy strand respectively;

[0017] 6) Aging treatment of aluminum alloy strands: Aging treatment is performed on the outermost aluminum alloy strands, the middle aluminum alloy strands, and the center aluminum alloy strands;

[0018] 7) Re-twisting: Re-twisting the outermost aluminum alloy strands, the middle aluminum alloy strands, and the center aluminum alloy strands after aging treatment according to the nominal cross-sectional size of the cable to obtain a re-twisted aluminum alloy conductor;

[0019] 8) Conductor aging treatment: Aluminum alloy conductor with disc is subjected to aging treatment to obtain torsion-resistant aluminum alloy wind power cable conductor;

[0020] 9) Cable production: Wrapping the outer layer of the torsion-resistant aluminum alloy wind power cable conductor with an insulating layer and a sheath as required to obtain the torsion-resistant aluminum alloy wind power cable.

[0021] Specifically, in the step 1), the aluminum alloy rod is manufactured through the following procedures: charging → melting → heat preservation → refining → filtering → continuous casting → shearing → continuous rolling → coiling.

[0022] Specifically, in step 1), the diameter of each aluminum alloy rod is 9.5 mm or 8.0 mm.

[0023] Preferably, in step 2), the aging treatment process is: the center layer aluminum alloy rod is placed in an aging furnace for aging treatment at 350-380°C for 2.5-3 hours; the middle layer aluminum alloy rod is placed in an aging furnace for aging treatment at 400-430°C for 3.5-4 hours; the outermost layer aluminum alloy rod is placed in an aging furnace for aging treatment at 430-450°C for 4-4.5 hours.

[0024] Preferably, in step 3), the three aluminum alloy rods after aging treatment are respectively drawn into aluminum alloy monofilaments with a diameter of 0.3 mm to 0.5 mm through three steps of aluminum alloy large drawing machine → medium drawing machine → small drawing machine or two steps of aluminum alloy large drawing machine → small drawing machine. The specific specifications are determined according to the conductor cross-section and the number of monofilaments required.

[0025] Preferably, in step 4), the aging treatment process is: the central layer aluminum alloy monofilament is subjected to aging treatment at 350-380°C for 3-3.5 hours; the middle layer aluminum alloy monofilament is subjected to aging treatment at 400-430°C for 4-4.5 hours; the outermost layer aluminum alloy monofilament is subjected to aging treatment at 430-450°C for 4-4.5 hours; after aging treatment, the tensile strength of the outermost layer aluminum alloy monofilament is 115-152MPa, and the elongation at break is ≥15%, the tensile strength of the middle layer aluminum alloy monofilament is ≥100MPa, and the elongation at break is ≥12%; the tensile strength of the central layer aluminum alloy monofilament is 115-152MPa, and the elongation at break is ≥12%.

[0026] Preferably, step 5) also includes: bundling the outermost aluminum alloy single wire, the middle aluminum alloy single wire, and the center aluminum alloy single wire after aging treatment into strands on a 500 bundle twisting machine, a 630 bundle twisting machine, or a 650 bundle twisting machine, respectively, to obtain the outermost aluminum alloy strand, the middle aluminum alloy strand, and the center aluminum alloy strand; wherein the amount of aluminum alloy single wire used in each strand is at least 16, the bundle pitch-diameter ratio is 15-20, and the bundle direction can be left or right.

[0027] Preferably, in step 6), the aging treatment process is: the center layer aluminum alloy strands are aged at 350-380°C for 2-2.5 hours; the middle layer aluminum alloy strands are aged at 400-430°C for 3-4 hours; the outermost layer aluminum alloy strands are aged at 430-450°C for 3.5-4 hours.

[0028] Preferably, in step 7), the outermost aluminum alloy strands, the middle aluminum alloy strands, and the center aluminum alloy strands after aging treatment are twisted in a total of 19-61 strands according to the nominal cross-sectional size of the cable; during the twisting, the strands are twisted in the same direction as the strands, the twisting directions of each layer are consistent, and the twisting pitch ratio is 10-14. During the twisting, the polyester reinforced non-woven fabric can be wrapped, and the polyester smooth surface of the polyester reinforced non-woven fabric faces inward, so as to facilitate the movement of the cable conductor during twisting.

[0029] Preferably, in step 8), the aging treatment temperature is 430-450° C., and the aging treatment time is 4-4.5 hours.

[0030] In some specific embodiments, in step 9), if the torsion-resistant alloy wind power cable is a single-core cable, an insulating layer and a sheath are wrapped around the outer layer of the torsion-resistant aluminum alloy wind power cable conductor to obtain the cable;

[0031] If the torsion-resistant alloy wind power cable is a multi-core cable, an insulating layer is wrapped around the torsion-resistant aluminum alloy wind power cable conductor to obtain an insulated core, and then the insulated core is cabled as needed and then wrapped with a sheath to obtain the cable.

[0032] Preferably, if the single-core cable is a single-core all-rubber cable, the insulation layer adopts EPDM insulation film for twist-resistant and low-temperature wind power cable or high-strength twist-resistant and highly flame-retardant cable insulation sheath film; the sheath material adopts chlorinated polyethylene sheath film for twist-resistant and low-temperature wind power cable or chloroprene rubber sheath film for twist-resistant and low-temperature wind power cable or chloroprene rubber sheath film for twist-resistant and low-temperature wind power cable or chlorosulfonated polyethylene sheath film for twist-resistant and low-temperature wind power cable or high-strength twist-resistant and highly flame-retardant cable insulation sheath film or polyurethane sheath material for twist-resistant and low-temperature wind power cable. The insulation layer and the sheath are double-layer co-extruded.

[0033] If the single-core cable is a single-core rubber-insulated plastic sheathed cable, the insulation layer adopts EPDM insulation film specially used for torsion-resistant and low-temperature-resistant wind power cables, and the sheath adopts polyurethane sheath material specially used for torsion-resistant and low-temperature-resistant wind power cables. The insulation layer and the sheath are extruded twice.

[0034] If the torsion-resistant alloy wind power cable is a multi-core cable, the insulation layer is extruded on a continuous vulcanization extruder unit using EPDM insulation film specially used for torsion-resistant and low-temperature wind power cables or high-strength torsion-resistant and highly flame-retardant cable insulation sheath film; the extruded insulation cores are cabled into multiple cores, and to ensure the torsional performance of the cable, the cabling pitch-diameter ratio is 12-14, the cabling direction is consistent with the conductor direction, no tape is wrapped during cabling, and the center is filled with rubber strips or hemp ropes; the sheath material is chlorinated polyethylene sheath film specially used for torsion-resistant and low-temperature wind power cables, or chloroprene rubber sheath film specially used for torsion-resistant and low-temperature wind power cables, or chloroprene rubber sheath film specially used for torsion-resistant and low-temperature wind power cables, or chlorosulfonated polyethylene sheath film specially used for torsion-resistant and low-temperature wind power cables, or high-strength torsion-resistant and highly flame-retardant cable insulation sheath film, or polyurethane sheath material specially used for torsion-resistant and low-temperature wind power cables.

[0035] The present invention improves the torsion resistance of aluminum alloy cables by improving the material formula of aluminum alloy strands and the preparation process of cable conductors. The specific principles are as follows:

[0036] 1. By improving the aluminum alloy formula of the outermost aluminum alloy strand, the tensile strength, toughness, heat resistance and corrosion resistance are improved. The principle is:

[0037] Adding silicon (Si) improves tensile strength, hardness, machinability, and tensile strength at high temperatures.

[0038] By adding copper, copper (Cu) is dissolved into the aluminum alloy to form AL-Cu, which improves the tensile strength of the outermost conductor.

[0039] Adding magnesium (Mg) to form an aluminum-magnesium alloy improves corrosion resistance.

[0040] By adding manganese (Mn), the recrystallization process of aluminum alloy is prevented, the recrystallization temperature is increased, and the recrystallized grains can be significantly refined. The refinement of recrystallized grains is mainly due to the MnAl6 compound dispersed particles hindering the growth of recrystallized grains. Another function of MnAl6 is to dissolve impure iron (Fe) to form (Fe, Mn)Al6 to reduce the harmful effects of iron.

[0041] Adding chromium (Cr) to aluminum forms intermetallic compounds such as (CrFe)Al7 and (CrMn)Al12, which improves the toughness of the alloy, reduces the sensitivity to stress corrosion cracking, and hinders the nucleation and growth process of recrystallization.

[0042] Adding zirconium Zr improves the tensile strength of the conductor, increases the alloy grain size, and makes it less likely for the wire to break during cable torsion.

[0043] Adding Sc improves the tensile strength, toughness, heat resistance and corrosion resistance of aluminum alloy. The outermost layer of the aluminum alloy conductor has a large torque during torsion, which requires greater tensile strength and toughness. At the same time, the outermost layer of aluminum alloy is in contact with vulcanized rubber, which requires higher heat resistance and corrosion resistance, ensuring that the outer layer of the conductor is not broken during torsion and has excellent heat resistance and corrosion resistance.

[0044] By adjusting the ratio of silicon, iron, copper, magnesium, chromium, zinc, boron, lithium, zirconium, Sn and Sc, the tensile strength and corrosion resistance of the conductor are improved, and the creep resistance of the aluminum alloy conductor at high temperature is improved, ensuring that the test temperature of the aluminum alloy conductor cable is 90°C, the compressive stress is 60-80MPa, the yield strength is 87-90MPa, and the creep strain of 100 hours is ≤0.4%.

[0045] 2. The torsional toughness of the outermost strands is improved through four aging treatments to solve the torsional toughness problem of the outermost conductor, namely, aging treatment of aluminum alloy rods, aging treatment of wire drawing into 0.3mm-0.5mm aluminum alloy, aging treatment after bundle twisting into strands, and aging treatment after re-twisting into conductors. The elongation at break of the outer layer monofilament is ≥15%.

[0046] 3. Through the aluminum alloy formula of the outermost strands and 4 aging treatments, it is ensured that the outer strands of the aluminum alloy wind power cable pass the torsion test without breaking during the 10,000-15,000 cycle room temperature torsion test.

[0047] 4. When the aluminum alloy wind power cable is twisted, the torque of the middle layer strands is small, and the probability of core breakage during actual twisting is small. The creep resistance and electrical properties are mainly considered during the formulation design. By adjusting the ratio of silicon, iron, copper, manganese, magnesium, zinc, boron, lithium, and Sc, the creep resistance and electrical properties of the aluminum alloy conductor at high temperature are improved, ensuring that the test temperature of the aluminum alloy conductor cable is 90°C, the compressive stress is 60-80MPa, the yield strength is 87-90MPa, and the creep strain of 100 hours is ≤0.4%.

[0048] 5. The center layer strands have the smallest torque when the aluminum alloy conductor wind power flexible cable is twisted, and they mainly bear the cable's own weight tension when twisted. The formula mainly considers tensile strength and creep resistance. By adjusting the ratio of silicon, iron, copper, magnesium, chromium, zinc, boron, lithium, tin Sn, and Sc, the tensile strength and corrosion resistance of the conductor are improved, and the creep resistance of the aluminum alloy conductor at high temperature is improved to ensure that the test temperature of the aluminum alloy conductor cable is 90°C, the compressive stress is 60-80MPa, the yield strength is 87-90MPa, and the creep strain of 100 hours is ≤0.4%.

[0049] The beneficial effects of the present invention are:

[0050] 1. Compared with the prior art, in order to solve the problem that the broken wires of the cable with a single 8030 aluminum alloy wire conductor are mainly the outermost strands during the torsion test, and the outer layer of the cable conductor is easy to break when torsion, the cable conductor of the present invention breaks through the use of aluminum alloy rods with two or three aluminum alloy formulas to respectively make the outer layer strands, middle layer strands and center layer strands of the conductor, thereby solving the problem that the outer layer strands are easy to break during the cable torsion test.

[0051] 2. Compared with the prior art, the outer layer of the cable conductor is prone to breakage during twisting. The outer layer strands of the conductor of the present invention adopt an aluminum alloy formula with high tensile strength, high toughness, heat resistance, corrosion resistance and creep resistance, focusing on improving the toughness of the conductor and enhancing the tensile strength, heat resistance and corrosion resistance, and solving the problem of broken wires in the outer layer during twisting.

[0052] 3. Compared with the prior art, the cable conductor of the present invention adopts four aging treatments, namely, aging treatment for aluminum alloy rods, aging treatment for drawing into 0.3mm-0.5mm single-filament aluminum alloy, aging treatment after twisting into strands, and aging treatment after twisting into conductors. This improves the toughness of the single-filament conductor and ensures that it can pass 11,000 cycles or 15,000 cycles of room-temperature torsion tests, solving the problem of aluminum alloy conductor torsion bottlenecks, and can overturn the pattern of using copper-core twisted cables in the torsion section of wind turbines, leading the market.

[0053] 4. Compared with the prior art, the aluminum alloy twisted cable provided by the present invention can replace the copper core twisted cable, and the material cost is reduced by more than 60%.

[0054] 5. Compared with the prior art, the present invention adopts three different aluminum alloy formulas for the conductor center layer, middle layer and outermost layer, and after four aging treatments, the cable current carrying capacity is increased by more than 15% compared with other aluminum alloy cables of the same specification at the same conductor operating temperature and ambient temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 This is a schematic diagram of the structure of a torsion-resistant aluminum alloy wind power cable (single core), where: 1-central layer aluminum alloy strands; 2-middle layer aluminum alloy strands; 3-outermost layer aluminum alloy strands; 4. polyester reinforced non-woven fabric; 5. insulation layer; 7. sheath;

[0056] Figure 2 It is a schematic diagram of the structure of a torsion-resistant aluminum alloy wind power cable (multi-core), wherein: 1-central layer aluminum alloy strands; 2-middle layer aluminum alloy strands; 3-outermost layer aluminum alloy strands; 4-polyester reinforced non-woven fabric; 5-insulating layer; 6-rubber strip or hemp rope; 7-sheath. DETAILED DESCRIPTION

[0057] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.

[0058] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0059] Example 1

[0060] 1. The aluminum alloy formula used in this embodiment is as follows:

[0061] The aluminum alloy formula of the outermost aluminum alloy strand is: by mass percentage, Si 0.45%, Fe 0.2%, Cu 0.03%, Mn 0.01%, Mg 0.4%, Cr 0.015%, Zn 0.009%, B 0.02%, Li 0.002%, Zr 0.003%, Sn 0.003%, Sc 0.016%, each impurity element ≤ 0.03%, the total amount of impurity elements ≤ 0.10%, and the rest is aluminum;

[0062] The aluminum alloy formula of the intermediate layer aluminum alloy strand is as follows: by mass percentage, Si 0.08%, Fe 0.3%, Cu 0.19%, Mg 0.001%, Zn 0.009%, B 0.01%, Li 0.001%, Sc 0.005%, each impurity element ≤ 0.03%, the total amount of impurity elements ≤ 0.10%, and the rest is aluminum;

[0063] The aluminum alloy formula of the center layer aluminum alloy strand is as follows: by mass percentage, Si 0.6%, Fe 0.25%, Cu0.01%, Mn 0.015%, Mg 0.45%, Cr 0.015%, Zn 0.009%, B 0.01%, Li 0.002%, Sn0.002%, Sc 0.016%, each impurity element ≤0.03%, the total amount of impurity elements ≤0.10%, and the rest is aluminum.

[0064] 2. Preparation of torsion-resistant aluminum alloy wind power cables:

[0065] 1) The outermost aluminum alloy rod is manufactured according to the aluminum alloy formula of the outermost aluminum alloy strand; the middle aluminum alloy rod is manufactured according to the aluminum alloy formula of the middle aluminum alloy strand; the center aluminum alloy rod is manufactured according to the aluminum alloy formula of the center aluminum alloy strand; wherein the diameters of the outermost aluminum alloy rod, the middle aluminum alloy rod and the center aluminum alloy rod are all 9.5 mm, and the rod manufacturing process is the conventional existing rod manufacturing process, specifically, charging → melting → heat preservation → refining → filtering → continuous casting → shearing → continuous rolling → coiling;

[0066] 2) performing aging treatment on the three aluminum alloy rods obtained in step 1), specifically: performing aging treatment on the center layer aluminum alloy rod at 350-380° C. for 2.5 hours, performing aging treatment on the middle layer aluminum alloy rod at 400-430° C. for 3 hours, and performing aging treatment on the outermost layer aluminum alloy rod at 430-450° C. for 4 hours;

[0067] 3) The three aluminum alloy rods with a diameter of 9.5 mm after the aging treatment in step 2) are respectively drawn into a center layer aluminum alloy monofilament, an intermediate layer aluminum alloy monofilament, and an outermost layer aluminum alloy monofilament with a diameter of 0.5 mm through an aluminum alloy large drawing machine, a medium drawing machine, and a small drawing machine;

[0068] 4) performing aging treatment on the three aluminum alloy monofilaments obtained in step 3), wherein the specific process is as follows: performing aging treatment on the center layer aluminum alloy monofilament at 350-380° C. for 3 hours, performing aging treatment on the middle layer aluminum alloy monofilament at 400-430° C. for 4 hours, and performing aging treatment on the outermost layer aluminum alloy monofilament at 430-450° C. for 4 hours;

[0069] 5) The three aluminum alloy monofilaments after aging treatment are bundled into strands on a 500 bundle stranding machine, and the bundle-stranded pitch ratio is 15-20, and the bundle-stranded direction is left-handed, respectively obtaining the outermost layer aluminum alloy strand, the middle layer aluminum alloy strand, and the center layer aluminum alloy strand;

[0070] 6) The three aluminum alloy strands are subjected to aging treatment respectively, and the process is as follows: the center layer aluminum alloy strand is subjected to aging treatment at 350-380° C. for 2 hours, the middle layer aluminum alloy strand is subjected to aging treatment at 400-430° C. for 3 hours, and the outermost layer aluminum alloy strand is subjected to aging treatment at 430-450° C. for 3.5 hours;

[0071] 7) According to the nominal cross-sectional size of the cable, the three types of aluminum alloy strands after aging treatment are re-twisted to obtain the re-twisted aluminum alloy conductor. During re-twisting, the strands are twisted in the same direction as the strands, and the twisting directions of each layer are consistent. The re-twisting section-diameter ratio is 10-14; during re-twisting, the polyester reinforced non-woven fabric is wrapped, and the polyester smooth surface of the polyester reinforced non-woven fabric faces inward, so as to facilitate the movement of the cable conductor when twisting;

[0072] 8) placing the reel of the re-twisted aluminum alloy conductor into an aging annealing furnace at 430-450° C. for aging treatment for 3.5 hours to obtain a torsion-resistant aluminum alloy wind power cable conductor;

[0073] 9) Cable preparation: The torsion-resistant aluminum alloy wind power cable conductor is made into a single-core cable with a specification of 1*400 by using existing technology, wherein the insulation layer is an EPDM insulation layer specially used for torsion-resistant and low-temperature wind power cables, and the sheath material is a chlorinated polyethylene sheath film specially used for torsion-resistant and low-temperature wind power cables.

[0074] Example 2

[0075] Compared with Example 1, the difference of this embodiment is:

[0076] 1. Aluminum alloy formula of the outermost aluminum alloy strand: by mass percentage, Si 0.6%, Fe 0.2%, Cu 0.05%, Mn 0.02%, Mg 0.4%, Cr 0.02%, Zn 0.010%, B 0.02%, Li 0.003%, Zr 0.01%, Sn 0.001%, Sc 0.02%, each impurity element ≤ 0.03%, the total amount of impurity elements ≤ 0.10%, and the rest is aluminum;

[0077] The aluminum alloy formula of the intermediate layer aluminum alloy strand is as follows: by mass percentage, Si 0.08%, Fe 0.3%, Cu 0.19%, Mg 0.001%, Zn 0.009%, B 0.01%, Li 0.005%, Sc 0.0015%, each impurity element ≤ 0.03%, the total amount of impurity elements ≤ 0.10%, and the rest is aluminum;

[0078] The aluminum alloy formula of the center layer aluminum alloy strand is as follows: by mass percentage, Si 0.6%, Fe 0.25%, Cu0.01%, Mn 0.015%, Mg 0.45%, Cr 0.015%, Zn 0.009%, B 0.01%, Li 0.003%, Sn0.001%, Sc 0.018%, each impurity element ≤0.03%, the total amount of impurity elements ≤0.10%, and the rest is aluminum.

[0079] 2. Aluminum alloy rod aging treatment process: the center layer aluminum alloy rod is aged at 350-380℃ for 3 hours, the middle layer aluminum alloy rod is aged at 400-430℃ for 3.5 hours, and the outermost layer aluminum alloy rod is aged at 430-450℃ for 4.5 hours;

[0080] Aluminum alloy monofilament aging treatment process: the center layer aluminum alloy monofilament is aged at 350-380℃ for 3.5 hours, the middle layer aluminum alloy monofilament is aged at 400-430℃ for 4.5 hours, and the outermost layer aluminum alloy monofilament is aged at 430-450℃ for 4 hours;

[0081] Aluminum alloy strand aging treatment process: the center layer aluminum alloy strand is aged at 350-380℃ for 2.5 hours, the middle layer aluminum alloy strand is aged at 400-430℃ for 3.5 hours, and the outermost layer aluminum alloy strand is aged at 430-450℃ for 4 hours;

[0082] Aluminum alloy conductor aging treatment process: 430-450℃ aging treatment for 4 hours;

[0083] The rest of the conditions remain unchanged.

[0084] Example 3

[0085] Compared with Example 2, the difference of this embodiment is only that:

[0086] Aluminum alloy strand aging treatment process: the center layer aluminum alloy strand is aged at 350-380℃ for 2.5 hours, the middle layer aluminum alloy strand is aged at 400-430℃ for 3.5 hours, and the outermost layer aluminum alloy strand is aged at 430-450℃ for 2.5 hours;

[0087] Aluminum alloy conductor aging treatment process: 430-450℃ aging treatment for 3.5 hours;

[0088] The other conditions remain unchanged. The results of the cable room temperature torsion test are shown in Table 1.

[0089] Example 4

[0090] Compared with Example 2, the only difference of this embodiment is that the specification of the cable is 1*300, and the other conditions remain unchanged.

[0091] Example 5

[0092] Compared with Example 2, the difference of this embodiment is only that:

[0093] Aluminum alloy conductor aging treatment process: 430-450℃ aging treatment for 3.5 hours;

[0094] The specification of the cable is 1*300; the other conditions remain unchanged.

[0095] Example 6

[0096] Compared with Example 2, the difference of this embodiment is only that:

[0097] The aluminum alloy formula of the outermost aluminum alloy strand is as follows: by mass percentage, Si 0.45%, Fe 0.2%, Cu 0.03%, Mn 0.01%, Mg 0.4%, Cr 0.015%, Zn 0.009%, B 0.02%, Li 0.003%, Zr 0.01%, Sn 0.001%, Sc 0.02%, each impurity element ≤ 0.03%, the total amount of impurity elements ≤ 0.10%, and the rest is aluminum;

[0098] Aluminum alloy conductor aging treatment process: 430-450℃ aging treatment for 3 hours;

[0099] The specification of the cable is 1*300;

[0100] The rest of the conditions remain unchanged.

[0101] Example 7

[0102] Compared with Example 1, the difference of this embodiment is only that:

[0103] The aluminum alloy formula of the outermost aluminum alloy strand is as follows: by mass percentage, Si 0.6%, Fe 0.2%, Cu 0.05%, Mn 0.02%, Mg 0.4%, Cr 0.02%, Zn 0.010%, B 0.02%, Li 0.003%, Zr 0.01%, Sn 0.001%, Sc 0.02%, each impurity element ≤ 0.03%, the total amount of impurity elements ≤ 0.10%, and the rest is aluminum;

[0104] The cable specification is 1*185; the diameter of the aluminum alloy wire is 0.40mm, and the other conditions remain unchanged.

[0105] The inventors conducted room temperature torsion tests on the cables prepared in Examples 1 to 7 and compared them with the existing conventional 8030 aluminum alloy cables. The specific results are shown in Table 1.

[0106] The existing conventional 8030 aluminum alloy cable adopts a single 8030 aluminum alloy formula for its aluminum alloy conductor, and only performs annealing and aging treatment on the conductor aluminum alloy rod and the aluminum alloy monofilament during its manufacturing process.

[0107] Table 1 Comparison of room temperature torsion test results of cables prepared in Examples 1 to 7 and conventional 8030 aluminum alloy cables

[0108] Test No. Specification Normal temperature torsion cycle (period) Passed Example 1 1*400 12000 pass Example 2 1*400 15000 pass Example 3 1*400 14000 pass Example 4 1*300 15000 pass Example 5 1*300 15000 pass Example 6 1*300 11000 pass Example 7 1*185 15000 pass 8030 aluminum alloy cable 1 1*300 10000 Not passed 8030 aluminum alloy cable 2 1*300 10000 Not passed 8030 aluminum alloy cable 3 1*400 10000 Not passed 8030 aluminum alloy cable 4 1*240 10000 Not passed 8030 aluminum alloy cable 5 1*240 10000 Not passed 8030 aluminum alloy cable 6 1*185 10000 pass 8030 aluminum alloy cable 7 1*185 10000 Not passed 8030 aluminum alloy cable 8 1*185 10000 Not passed 8030 aluminum alloy cable 9 1*185 10000 Not passed 8030 aluminum alloy cable 10 1*240 10000 Not passed

[0109] It can be seen from the data in Table 1 that the present invention has the following advantages over conventional aluminum alloy conductor processes in the cable industry: the pass rate of the room temperature torsion test is improved from 10% in the original 10,000 cycles of room temperature torsion to 100% in 11,000 cycles of room temperature torsion, and even 15,000 cycles of room temperature torsion can be passed after aging treatment.

Claims

1. A torsion-resistant aluminum alloy wind power cable, comprising an aluminum alloy conductor, It is characterized in that The aluminum alloy conductor comprises an outermost aluminum alloy strand, an intermediate aluminum alloy strand and a center aluminum alloy strand; the aluminum alloy formula of the outermost aluminum alloy strand comprises the following components by mass percentage: Si 0.4%-0.6%, Fe 0.1%-0.3%, Cu 0.02%-0.05%, Mn0.01%-0.02%, Mg 0.35%-0.5%, Cr 0.01%-0.02%, Zn≤0.10%, B 0.01%-0.05%, Li 0.001%-0.005%, Zr 0.003%-0.01%, Sn 0.001%- 0.005%, Sc 0.016%-0.02%, each impurity element is ≤0.03%, the total amount of impurity elements is ≤0.10%, and the rest is aluminum; The aluminum alloy formula of the intermediate layer aluminum alloy strand includes the following components by mass percentage: Si 0.05%-0.1%, Fe 0.3%-0.4%, Cu 0.10%-0.20%, Mg 0.001%-0.005%, Zn 0.005%-0.01%, B 0.001%-0.01%, Li 0.001%-0.005%, Sc 0.0015%-0.017%, each impurity element ≤0.03%, the total amount of impurity elements ≤0.10%, and the rest is aluminum; The aluminum alloy formula of the center layer aluminum alloy strand is: the following components are included by mass percentage: Si 0.05%-0.1%, Fe 0.3%-0.4%, Cu 0.10%-0.20%, Mg 0.001%-0.005%, Zn 0.005%-0.01%, B 0.001%-0.01%, Li 0.001%-0.005%, Sc 0.0015%-0.017%, each impurity element is ≤0.03%, the total amount of impurity elements is ≤0.10%, and the rest is aluminum; Or includes the following components by mass percentage: Si 0.6%-0.7%, Fe 0.2%-0.3%, Cu 0.01%-0.015%, Mn0.01%-0.02%, Mg 0.35%-0.5%, Cr 0.01%-0.02%, Zn≤0.10%, B 0.01%-0.05%, Li 0.001%-0.005%, Sn 0.001%-0.005%, Sc 0.016%-0.020%, each impurity element ≤0.03%, the total amount of impurity elements ≤0.10%, and the rest is aluminum.

2. A method for manufacturing a torsion-resistant aluminum alloy wind power cable as claimed in claim 1, comprising the following steps: 1) Manufacturing aluminum alloy rods: the outermost aluminum alloy rod is manufactured according to the aluminum alloy formula used for the outermost aluminum alloy strands; the middle layer aluminum alloy rod is manufactured according to the aluminum alloy formula used for the middle layer aluminum alloy strands; the center layer aluminum alloy rod is manufactured according to the aluminum alloy formula used for the center layer aluminum alloy strands; 2) Aging treatment of aluminum alloy rods: Aging treatment is performed on the outermost aluminum alloy rod, the middle layer aluminum alloy rod, and the center layer aluminum alloy rod respectively; 3) Aluminum alloy monofilament drawing: the outermost aluminum alloy rod, the middle aluminum alloy rod and the center aluminum alloy rod after aging treatment are drawn into the outermost aluminum alloy monofilament, the middle aluminum alloy monofilament and the center aluminum alloy monofilament respectively; 4) Aging treatment of aluminum alloy monofilaments: Aging treatment is performed on the outermost layer aluminum alloy monofilaments, the middle layer aluminum alloy monofilaments, and the center layer aluminum alloy monofilaments respectively; 5) Aluminum alloy monofilament bundle twisting: The outermost aluminum alloy monofilament, the middle aluminum alloy monofilament and the center aluminum alloy monofilament after aging treatment are bundled into strands on a bundle twisting machine to obtain the outermost aluminum alloy strand, the middle aluminum alloy strand and the center aluminum alloy strand; 6) Aging treatment of aluminum alloy strands: Aging treatment is performed on the outermost aluminum alloy strands, the middle aluminum alloy strands, and the center aluminum alloy strands; 7) Re-twisting: According to the nominal cross-sectional size of the cable, the outermost aluminum alloy strands, the middle aluminum alloy strands and the center aluminum alloy strands after aging treatment are re-twisted to obtain the re-twisted aluminum alloy conductor; 8) Conductor aging treatment: Aluminum alloy conductor with disc is subjected to aging treatment to obtain torsion-resistant aluminum alloy wind power cable conductor; 9) Cable insulation and sheath production: Wrap an insulating layer and a sheath on the outer layer of the torsion-resistant aluminum alloy wind power cable conductor as required to obtain the torsion-resistant aluminum alloy wind power cable.

3. The manufacturing method according to claim 2, It is characterized in that In step 2), the aging treatment process is as follows: the center layer aluminum alloy rod is placed in an aging furnace at 350-380°C for aging treatment for 2.5-3 hours; the middle layer aluminum alloy rod is placed in an aging furnace at 400-430°C for aging treatment for 3.5-4 hours; the outermost layer aluminum alloy rod is placed in an aging furnace at 430-450°C for aging treatment for 4-4.5 hours.

4. The manufacturing method according to claim 2, It is characterized in that In step 4), the aging treatment process is as follows: the central layer aluminum alloy single wire is subjected to aging treatment at 350-380°C for 3-3.5 hours; the middle layer aluminum alloy single wire is subjected to aging treatment at 400-430°C for 4-4.5 hours; the outermost layer aluminum alloy single wire is subjected to aging treatment at 430-450°C for 4-4.5 hours; after aging treatment, the tensile strength of the outermost layer aluminum alloy single wire is 115-152MPa, and the elongation at break is ≥15%, the tensile strength of the middle layer aluminum alloy single wire is ≥100MPa, and the elongation at break is ≥12%; the tensile strength of the central layer aluminum alloy single wire is 115-152MPa, and the elongation at break is ≥12%.

5. The manufacturing method according to claim 2, It is characterized in that In step 6), the aging treatment process is as follows: the center layer aluminum alloy strands are aged at 350-380°C for 2-2.5 hours; the middle layer aluminum alloy strands are aged at 400-430°C for 3-4 hours; and the outermost layer aluminum alloy strands are aged at 430-450°C for 3.5-4 hours.

6. The manufacturing method according to claim 2, It is characterized in that In step 8), the temperature of the aging treatment of the aluminum alloy conductor is 430-450° C., and the aging treatment time is 4-4.5 hours.

7. The manufacturing method according to claim 2, It is characterized in that In step 3), the diameters of the outermost aluminum alloy monofilament, the middle aluminum alloy monofilament, and the center aluminum alloy monofilament are all 0.3 mm to 0.5 mm.

8. The manufacturing method according to claim 2, It is characterized in that In step 7), the outermost aluminum alloy strands, the middle aluminum alloy strands, and the center aluminum alloy strands after aging treatment are twisted again according to the nominal cross-sectional size of the cable, totaling 19-61 strands; during the twisting, the strands are twisted in the same direction as the strands, and the twisting directions of each layer are consistent.