A corrosion-resistant power cable and a method for preparing the same
By using modified fillers and modified epoxy resin coatings in the sheath and corrosion protection layer of the cable, combined with nanomaterials and electrostatic self-assembly technology, the problem of cable corrosion in humid or acid-base environments is solved, and excellent Corrosion resistance and flame retardant properties extend cable life and improve safety.
Patent Information
- Application Number
- CN202410322807.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-03-20
AI Technical Summary
Power cables are prone to corrosion in humid or acid-base environments, resulting in shortening of service life and frequent fire accidents, requiring improved corrosion resistance and flame retardant performance of the cable.
Modified fillers and modified epoxy resin coatings are used to improve the corrosion resistance of cables by adding boron nitride nanotubes, MXene nanosheets and carbon quantum dots to the sheath and corrosion protection layer. Flame retardant properties and enhance the density and hydrophobicity of the coating by modification treatment of epoxy resin.
It significantly improves the corrosion resistance and flame retardant properties of the cable, can maintain stability in an acid-base environment, extend the cable life, and form a dense carbon layer structure during the combustion process to inhibit continuous combustion.
Smart Images

Figure BDA0004751007950000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of power cables, and in particular to a corrosion-resistant power cable and a preparation method thereof. Background Art
[0002] The basic structure of power cable consists of four parts: core (conductor), insulation layer, shielding layer and sheath layer. The function of the sheath layer is to protect the power cable from the intrusion of external impurities and moisture, and to prevent external forces from directly damaging the power cable. However, due to the wide area of laying power cables, when laying power cables in some humid areas or acidic or alkaline environments, power cables are more susceptible to corrosion, which not only greatly affects the function of the cable but also shortens the service life of the cable.
[0003] At present, the method to improve the corrosion resistance of power cables is usually to apply a layer of anti-corrosion coating on the outer surface of the cable, such as acrylic coating, polyurethane coating, epoxy resin coating, etc. However, although such coatings have certain corrosion resistance, they are far from meeting actual needs and need to be modified to improve corrosion resistance. In addition, the sheath layer can also be treated to make it corrosion-resistant, and a double-layer protection method can be used to improve the corrosion resistance of power cables. In addition, fire accidents caused by cable fires are becoming more and more frequent, which has led to higher and higher requirements for the flame retardant properties of cables. Therefore, developing a power cable with excellent corrosion resistance and flame retardancy is one of the problems that need to be solved urgently. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a corrosion-resistant power cable and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A corrosion-resistant power cable comprises an anti-corrosion layer, a sheath layer arranged inside the anti-corrosion layer, an insulating layer arranged inside the sheath layer, a shielding layer arranged inside the insulating layer, and a conductor arranged inside the shielding layer;
[0007] The conductor is a copper conductor, the shielding layer is an aluminum-plastic composite tape shielding layer, the insulating layer is polyvinyl chloride, the sheath layer is made of sheath material, and the anti-corrosion layer is coated with epoxy resin paint;
[0008] The sheath material is prepared by the following steps:
[0009] Step A1, stirring and mixing boron nitride nanotubes and tris(hydroxymethyl)aminomethane) in a mixture of ethanol, methanol and deionized water, recorded as solution A; then dispersing dopamine hydrochloride in deionized water, recorded as solution B; then pouring solution B into solution A for ultrasonic dispersion for 10-20 minutes, and reacting for 8-12 hours under stirring conditions, after the reaction is completed, centrifuging, washing, and vacuum drying at 70°C for 10 hours to obtain BNNTs@PDA nanomaterials;
[0010] Furthermore, the dosage ratio of boron nitride nanotubes, tris(hydroxymethyl)aminomethane, ethanol, methanol and deionized water in solution A is 0.2-0.4 g: 0.15-0.45 g: 50 mL: 50 mL: 100 mL; and the dosage ratio of dopamine hydrochloride and deionized water in solution B is 0.8-2.0 g: 100 mL.
[0011] Step A2, ultrasonically disperse the MXene nanosheets after HCl-LiF etching in deionized water for 30 minutes, centrifuge to obtain the supernatant, add citric acid and polyethylene glycol to the supernatant and stir to mix evenly, transfer the resulting mixed solution to a reactor, react at 160-180°C for 3-5 hours, after the reaction is completed, cool to room temperature, centrifuge, wash, redisperse the precipitate in 10 mL of deionized water, add thioglycolic acid with a pH of 7, stir to react for 20-40 minutes, centrifuge, wash, and dry to obtain MPA-C QDs / MXene nanomaterials;
[0012] Further, the dosage ratio of MXene nanosheets, citric acid, polyethylene glycol, deionized water, and thioglycolic acid is 0.1-0.5 g: 2-3 g: 10 mL: 20 mL: 0.5-3 mL;
[0013] Furthermore, the pH of thioglycolic acid was adjusted using 4 mol / L sodium hydroxide solution.
[0014] Step A3, dispersing BNNTs@PDA nanomaterials in deionized water, adjusting the pH to 6-6.5, adding MPA-C QDs / MXene nanomaterials, and oscillating for 12 hours using a constant temperature oscillator. After the reaction is completed, centrifuging, washing, and freeze-drying to obtain a modified filler;
[0015] Furthermore, the dosage ratio of BNNTs@PDA nanomaterial, MPA-C QDs / MXene nanomaterial and deionized water is 0.5-1 g: 0.2-0.4 g: 20 mL.
[0016] Step A4, weigh the raw materials by weight, add 40-60 parts of polyvinyl chloride, 20-30 parts of silicone rubber, 10-15 parts of ACR toughener, 3-5 parts of vulcanizer, 1-2 parts of vulcanization accelerator, 2-4 parts of lubricant, 5-8 parts of diethyl phthalate, 5-10 parts of modified filler and 0.5-1 part of antioxidant into a double-roll plasticizer, and mix at 120-140° C. for 30 minutes, then place the mixed rubber on a flat vulcanizer, set the temperature to 200-220° C., preheat for 30 minutes, then press vulcanize at 10 MPa for 3-5 minutes, cool, and obtain the sheath material.
[0017] The epoxy resin coating is prepared by the following steps:
[0018] Step B1, add perfluorohexylethyl acrylate and 5-hexenylmethyldichlorosilane into a flask and mix evenly, then add dibenzoyl peroxide and diethylene glycol dimethyl ether, then introduce nitrogen into the system, and heat the system to 80-95° C. to react for 6-8 hours. After the reaction is completed, cool to 60° C., then add butyl acetate and deionized water, wash and separate, and then dry the precipitate at 60° C. for 5 hours to obtain a fluorine-containing resin;
[0019] Furthermore, the usage ratio of perfluorohexylethyl acrylate, 5-hexenyltrimethoxysilane, dibenzoyl peroxide, diethylene glycol dimethyl ether, butyl acetate and deionized water is 1-3 g: 2-3 g: 0.05 g: 4-6 mL: 5 mL: 15 mL.
[0020] Step B2, add epoxy resin E51 and butyl acetate into a flask, heat to 50°C and stir for 30 minutes, then add fluorine-containing resin, dibutyltin dilaurate and triethylamine in sequence, continue stirring and react for 6-8 hours, after the reaction is completed, centrifuge, wash 3-5 times, and then distill under reduced pressure to obtain a modified epoxy resin;
[0021] Furthermore, the usage ratio of epoxy resin E51, butyl acetate, fluorine-containing resin, dibutyltin dilaurate and triethylamine is 30-40 g: 15-20 mL: 1.5-3.5 g: 0.2-0.3 g: 10 g.
[0022] Step B3, weigh the raw materials by weight, add 30-40 parts of modified epoxy resin and 7-10 parts of ceramic powder into a ball mill and ball mill at a speed of 300-400rpm for 1-2h, then add 0.1-0.3 parts of defoaming agent and 15-25 parts of deionized water in a high-speed rotary machine and stir at a speed of 800-1000rpm for 20min, finally add 0.2-0.5 parts of leveling agent, 1-5 parts of curing agent, 0.5-0.8 parts of antistatic agent and 0.1-0.3 parts of thickener and continue stirring for 30min to obtain epoxy resin coating.
[0023] A method for preparing a corrosion-resistant power cable comprises the following steps:
[0024] An aluminum-plastic composite tape is wrapped around the copper conductor to form a shielding layer; polyvinyl chloride is then extruded outside the shielding layer to form an insulating layer; a sheath material is then extruded outside the insulating layer to form a sheath layer; finally, 50-70 μm of the epoxy resin coating prepared in Example 3 is evenly coated on the outside of the sheath layer to form an anti-corrosion layer, thereby obtaining a corrosion-resistant power cable.
[0025] Beneficial effects of the present invention:
[0026] The corrosion-resistant power cable prepared by the present invention comprises an anti-corrosion layer, a sheath layer arranged in the anti-corrosion layer, an insulating layer arranged in the sheath layer, a shielding layer arranged in the insulating layer, and a conductor arranged in the shielding layer; the conductor is a copper conductor, the shielding layer is an aluminum-plastic composite tape shielding layer, the insulating layer is polyvinyl chloride, and the sheath layer is prepared from a sheath material, which is mainly made of polyvinyl chloride and silicone rubber with excellent corrosion resistance, and then modified fillers are added to improve the corrosion resistance and flame retardant properties of the matrix; the anti-corrosion layer is coated with a modified epoxy resin coating, which further improves the corrosion resistance of the matrix.
[0027] In the modified filler, first, boron nitride nanotubes were used as the substrate, and a layer of polydopamine was coated on the surface to synthesize BNNTs@PDA nanomaterials; secondly, citric acid was used as the carbon source, and carbon quantum dots were synthesized on MXene nanosheets etched by HCl-LiF by hydrothermal reaction, and thioglycolic acid was modified on the surface of the quantum dots to synthesize MPA-C QDs / MXene nanomaterials; finally, the protonated positively charged BNNTs@PDA nanomaterials and the negatively charged MPA-CQDs / MXene nanomaterials were self-assembled into modified fillers by electrostatic self-assembly, which improved the corrosion resistance and flame retardancy of the matrix. In this filler: 1) Boron nitride nanotubes and polydopamine coated on their surface work together to improve the corrosion resistance of the matrix. Among them, boron nitride nanotubes have good chemical stability, so they can remain stable in acid, alkaline and neutral environments; the polydopamine coating on its surface avoids the agglomeration of boron nitride nanotubes in the matrix due to intermolecular forces, and improves the dispersibility of boron nitride nanotubes in the matrix; the presence of polydopamine also further improves the corrosion resistance of the matrix; in addition, due to the presence of a large number of amino groups in polydopamine, under acidic conditions, polydopamine is positively charged due to the protonation of the amino groups. 2) Using citric acid as a carbon source, carbon quantum dots are synthesized on MXene nanosheets etched with HCl-LiF by hydrothermal reaction, which improves the dispersibility of MXene nanosheets and increases the specific surface area of MPA-C QDs / MXene nanomaterials, and then the thiol groups in thioglycolic acid are used to modify the surface of the quantum dots, so that MPA-C The negative potential of QDs / MXene nanomaterials increases; among them, MXene nanosheets have a two-dimensional layered structure, and its unique structure has excellent barrier properties, which can effectively resist the invasion of oxygen and water molecules in the air, thereby improving the corrosion resistance of the matrix; in addition, MXene nanosheets and carbon quantum dots also work synergistically to improve the flame retardant properties of the matrix. This is because MXene nanosheets and their decomposition product TiO2 have good physical barrier effects during the combustion process, forming a "maze" in the matrix, extending the diffusion path of the gas, thereby inhibiting the continuous combustion of the matrix. Its decomposition product TiO2 also has excellent catalytic activity, which can promote the carbonization of polymers in the matrix, and play a good catalytic carbonization and smoke suppression role, while carbon quantum dots will form a dense carbon layer structure during combustion, thereby preventing further combustion of the matrix.
[0028] In the epoxy resin coating, firstly, perfluorohexylethyl acrylate and 5-hexenylmethyldichlorosilane are used as raw materials, and dibenzoyl peroxide is used as an initiator to synthesize a fluorine-containing resin; secondly, the -Cl group contained in the fluorine-containing resin reacts with the hydroxyl group in the epoxy resin, and the fluorine-containing resin is grafted on the epoxy resin to synthesize a modified epoxy resin. The fluorine-containing groups in the epoxy resin coating tend to migrate to the film surface during the film formation process, resulting in the enrichment of fluorine elements on the film surface, improving the hydrophobicity of the coating surface, and then preventing corrosive substances in the air from entering the matrix, thereby improving the corrosion resistance of the matrix; in addition, the fluorine-containing resin will also cross-link with the epoxy resin molecular chain during the film formation process, increasing the cross-linking density of the matrix, making the coating denser, and further inhibiting the corrosion of the matrix by corrosive substances. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] 1) The sheath material is prepared by the following steps:
[0032] Step A1, 0.2g of boron nitride nanotubes and 0.15g of tris(hydroxymethyl)aminomethane) were stirred and mixed in a mixture of 50mL of ethanol, 50mL of methanol and 100mL of deionized water, which was recorded as solution A; 0.8g of dopamine hydrochloride was evenly dispersed in 100mL of deionized water, which was recorded as solution B; then solution B was poured into solution A for ultrasonic dispersion for 10min, and reacted for 8h under stirring conditions. After the reaction was completed, centrifugation, washing, and vacuum drying at 70°C for 10h were obtained to obtain BNNTs@PDA nanomaterials;
[0033] Step A2, ultrasonically disperse 0.1g of MXene nanosheets after HCl-LiF etching in 20mL of deionized water for 30min, centrifuge to obtain the supernatant, add 2g of citric acid and 10mL of polyethylene glycol to the supernatant and stir to mix evenly, transfer the resulting mixture to a reactor, react at 160°C for 3h, after the reaction is completed, cool to room temperature, centrifuge, wash, and redisperse the precipitate in 10mL of deionized water, and then add 0.5mL of thioglycolic acid with a pH of 7, stir to react for 20min, centrifuge, wash, and dry to obtain MPA-C QDs / MXene nanomaterials, and adjust the pH of thioglycolic acid with a 4mol / L sodium hydroxide solution;
[0034] Step A3, 0.5 g of BNNTs@PDA nanomaterial was dispersed in 20 mL of deionized water, and the pH was adjusted to 6, and then 0.2 g of MPA-C QDs / MXene nanomaterial was added, and the mixture was oscillated on a constant temperature oscillator for 12 h. After the reaction was completed, the mixture was centrifuged, washed, and freeze-dried to obtain a modified filler;
[0035] Step A4, weigh the raw materials by weight, add 40 parts of polyvinyl chloride, 20 parts of silicone rubber, 10 parts of ACR toughener, 3 parts of N, N'-m-phenylene bismaleimide, 1 part of vulcanization accelerator NA-22, 2 parts of zinc stearate, 5 parts of diethyl phthalate, 5 parts of modified filler and 0.5 parts of antioxidant 1010 into a double-roll plasticizer, and mix at 120 ° C for 30 minutes, then place the mixed rubber on a flat vulcanizer, set the temperature to 200 ° C, preheat for 30 minutes, and then press vulcanize at 10 MPa for 3 minutes, cool, and obtain the sheath material.
[0036] 2) Epoxy resin coating, prepared by the following steps:
[0037] Step B1, add 1g of perfluorohexylethyl acrylate and 2g of 5-hexenylmethyldichlorosilane into a flask and mix evenly, then add 0.05g of dibenzoyl peroxide and 4mL of diethylene glycol dimethyl ether, then introduce nitrogen into the system, and heat the system to 80°C for reaction for 6h. After the reaction is completed, cool to 60°C, add 5mL of butyl acetate and 15mL of deionized water, wash and separate, and then dry the precipitate at 60°C for 5h to obtain a fluorine-containing resin;
[0038] Step B2, add 30g epoxy resin E51 and 15mL butyl acetate into a flask, heat to 50°C and stir for 30min, then add 1.5g fluorine-containing resin, 0.2g dibutyltin dilaurate and 10g triethylamine in sequence, continue stirring and react for 6h, after the reaction is completed, centrifuge and wash 3 times, and then distill under reduced pressure to obtain a modified epoxy resin;
[0039] Step B3, weigh the raw materials by weight, add 30 parts of modified epoxy resin and 7 parts of ceramic powder into a ball mill and ball mill at 300 rpm for 1 hour, then add 0.1 parts of dimethyl silicone oil and 15 parts of deionized water in a high-speed rotary machine and stir at 800 rpm for 20 minutes, finally add 0.2 parts of hydroxymethyl cellulose, 1 part of trimethylhexamethylenediamine, 0.5 parts of antistatic agent SH-105 and 0.1 parts of acrylic thickener and continue stirring for 30 minutes to obtain the epoxy resin coating.
[0040] Example 2
[0041] 1) The sheath material is prepared by the following steps:
[0042] Step A1, 0.3g of boron nitride nanotubes and 0.25g of tris(hydroxymethyl)aminomethane) were stirred and mixed in a mixture of 50mL of ethanol, 50mL of methanol and 100mL of deionized water, which was recorded as solution A; 1.5g of dopamine hydrochloride was evenly dispersed in 100mL of deionized water, which was recorded as solution B; then solution B was poured into solution A for ultrasonic dispersion for 15min, and reacted for 10h under stirring conditions. After the reaction was completed, centrifugation, washing, and vacuum drying at 70°C for 10h were performed to obtain BNNTs@PDA nanomaterials;
[0043] Step A2, ultrasonically disperse 0.3g of MXene nanosheets after HCl-LiF etching in 20mL of deionized water for 30min, centrifuge to obtain the supernatant, add 2.5g of citric acid and 10mL of polyethylene glycol to the supernatant and stir to mix evenly, transfer the resulting mixture to a reactor, react at 170°C for 4h, after the reaction is completed, cool to room temperature, centrifuge, wash, and redisperse the precipitate in 10mL of deionized water, and then add 1.5mL of thioglycolic acid with a pH of 7, stir to react for 30min, centrifuge, wash, and dry to obtain MPA-C QDs / MXene nanomaterials, and adjust the pH of thioglycolic acid with a 4mol / L sodium hydroxide solution;
[0044] Step A3, 0.8 g of BNNTs@PDA nanomaterial was dispersed in 20 mL of deionized water, and the pH was adjusted to 6, and then 0.3 g of MPA-C QDs / MXene nanomaterial was added, and the mixture was oscillated on a constant temperature oscillator for 12 h. After the reaction was completed, the mixture was centrifuged, washed, and freeze-dried to obtain a modified filler;
[0045] Step A4, weigh the raw materials by weight, add 50 parts of polyvinyl chloride, 25 parts of silicone rubber, 13 parts of ACR toughener, 4 parts of N, N'-m-phenylene bismaleimide, 1.5 parts of vulcanization accelerator NA-22, 3 parts of zinc stearate, 7 parts of diethyl phthalate, 8 parts of modified filler and 0.8 parts of antioxidant 1010 into a double-roll plasticizer, and mix at 130 ° C for 30 minutes, then place the mixed rubber on a flat vulcanizer, set the temperature to 210 ° C, preheat for 30 minutes, and then press vulcanize at 10 MPa for 5 minutes, cool, and obtain the sheath material.
[0046] 2) Epoxy resin coating, prepared by the following steps:
[0047] Step B1, add 2g of perfluorohexylethyl acrylate and 2.5g of 5-hexenylmethyldichlorosilane into a flask and mix evenly, then add 0.05g of dibenzoyl peroxide and 5mL of diethylene glycol dimethyl ether, then introduce nitrogen into the system, and heat the system to 90°C for reaction for 7h. After the reaction is completed, cool to 60°C, add 5mL of butyl acetate and 15mL of deionized water, wash and separate, and then dry the precipitate at 60°C for 5h to obtain a fluorine-containing resin;
[0048] Step B2, add 35g epoxy resin E51 and 17mL butyl acetate into a flask, heat to 50°C and stir for 30min, then add 2.5g fluorine-containing resin, 0.25g dibutyltin dilaurate and 10g triethylamine in sequence, continue stirring and react for 7h, after the reaction is completed, centrifuge and wash 3 times, and then distill under reduced pressure to obtain a modified epoxy resin;
[0049] Step B3, weigh the raw materials by weight, add 35 parts of modified epoxy resin and 8 parts of ceramic powder into a ball mill and ball mill at 300 rpm for 1.5 hours, then add 0.2 parts of dimethyl silicone oil and 20 parts of deionized water in a high-speed rotary machine and stir at 900 rpm for 20 minutes, finally add 0.3 parts of hydroxymethyl cellulose, 3 parts of trimethylhexanediamine, 0.7 parts of antistatic agent SH-105 and 0.2 parts of acrylic thickener and continue stirring for 30 minutes to obtain the epoxy resin coating.
[0050] Example 3
[0051] 1) The sheath material is prepared by the following steps:
[0052] Step A1, 0.4g of boron nitride nanotubes and 0.45g of tris(hydroxymethyl)aminomethane) were stirred and mixed in a mixture of 50mL of ethanol, 50mL of methanol and 100mL of deionized water, which was recorded as solution A; 2.0g of dopamine hydrochloride was evenly dispersed in 100mL of deionized water, which was recorded as solution B; then solution B was poured into solution A for ultrasonic dispersion for 20min, and reacted for 12h under stirring conditions. After the reaction was completed, centrifugation, washing, and vacuum drying at 70°C for 10h were performed to obtain BNNTs@PDA nanomaterials;
[0053] Step A2, ultrasonically disperse 0.5g of MXene nanosheets after HCl-LiF etching in 20mL of deionized water for 30min, centrifuge to obtain the supernatant, add 3g of citric acid and 10mL of polyethylene glycol to the supernatant and stir to mix evenly, transfer the resulting mixture to a reactor, react at 180°C for 5h, after the reaction is completed, cool to room temperature, centrifuge, wash, and redisperse the precipitate in 10mL of deionized water, and then add 3mL of thioglycolic acid with a pH of 7, stir to react for 40min, centrifuge, wash, and dry to obtain MPA-C QDs / MXene nanomaterials, and adjust the pH of thioglycolic acid with a 4mol / L sodium hydroxide solution;
[0054] Step A3, disperse 1g of BNNTs@PDA nanomaterial in 20mL of deionized water, adjust the pH to 6.5, add 0.4g of MPA-C QDs / MXene nanomaterial, and oscillate for 12h using a constant temperature oscillator. After the reaction is completed, centrifuge, wash, and freeze-dry to obtain a modified filler;
[0055] Step A4, weigh the raw materials by weight, add 60 parts of polyvinyl chloride, 30 parts of silicone rubber, 15 parts of ACR toughener, 5 parts of N, N'-phenylene bismaleimide, 2 parts of vulcanization accelerator NA-22, 4 parts of zinc stearate, 8 parts of diethyl phthalate, 10 parts of modified filler and 1 part of antioxidant 1010 into a double-roll plasticizer, and mix at 140 ° C for 30 minutes, then place the mixed rubber on a flat vulcanizer, set the temperature to 220 ° C, preheat for 30 minutes, and then press vulcanize at 10 MPa for 5 minutes, cool, and obtain the sheath material.
[0056] 2) Epoxy resin coating, prepared by the following steps:
[0057] Step B1, add 3g of perfluorohexylethyl acrylate and 3g of 5-hexenylmethyldichlorosilane into a flask and mix evenly, then add 0.05g of dibenzoyl peroxide and 6mL of diethylene glycol dimethyl ether, then introduce nitrogen into the system, and heat the system to 95°C for reaction for 8h. After the reaction is completed, cool to 60°C, add 5mL of butyl acetate and 15mL of deionized water, wash and separate, and then dry the precipitate at 60°C for 5h to obtain a fluorine-containing resin;
[0058] Step B2, add 40g epoxy resin E51 and 20mL butyl acetate into a flask, heat to 50°C and stir for 30min, then add 3.5g fluorine-containing resin, 0.3g dibutyltin dilaurate and 10g triethylamine in sequence, continue stirring and react for 8h, after the reaction is completed, centrifuge and wash 5 times, and then distill under reduced pressure to obtain a modified epoxy resin;
[0059] Step B3, weigh the raw materials by weight, add 40 parts of modified epoxy resin and 10 parts of ceramic powder into a ball mill and ball mill at 400 rpm for 2 hours, then add 0.3 parts of dimethyl silicone oil and 25 parts of deionized water in a high-speed rotary machine and stir at 1000 rpm for 20 minutes, finally add 0.5 parts of hydroxymethyl cellulose, 5 parts of trimethylhexanediamine, 0.8 parts of antistatic agent SH-105 and 0.3 parts of acrylic thickener and continue stirring for 30 minutes to obtain the epoxy resin coating.
[0060] Example 4
[0061] A corrosion-resistant power cable comprises an anti-corrosion layer, a sheath layer arranged in the anti-corrosion layer, an insulating layer arranged in the sheath layer, a shielding layer arranged in the insulating layer, and a conductor arranged in the shielding layer; the conductor is a copper conductor, the shielding layer is an aluminum-plastic composite tape shielding layer, the insulating layer is polyvinyl chloride, the sheath layer is prepared by the sheath material prepared in Example 1, and the anti-corrosion layer is coated with the epoxy resin coating prepared in Example 1, and specifically comprises the following steps:
[0062] An aluminum-plastic composite tape is wrapped around the copper conductor to form a shielding layer; polyvinyl chloride is extruded outside the shielding layer to form an insulating layer; the sheath material prepared in Example 1 is extruded outside the insulating layer to form a sheath layer; finally, 50 μm of the epoxy resin coating prepared in Example 3 is evenly coated on the outside of the sheath layer to form an anti-corrosion layer, thereby obtaining a corrosion-resistant power cable.
[0063] Example 5
[0064] A corrosion-resistant power cable comprises an anti-corrosion layer, a sheath layer arranged in the anti-corrosion layer, an insulating layer arranged in the sheath layer, a shielding layer arranged in the insulating layer, and a conductor arranged in the shielding layer; the conductor is a copper conductor, the shielding layer is an aluminum-plastic composite tape shielding layer, the insulating layer is polyvinyl chloride, the sheath layer is prepared by the sheath material prepared in Example 2, and the anti-corrosion layer is coated with the epoxy resin coating prepared in Example 2, specifically comprising the following steps:
[0065] An aluminum-plastic composite tape is wrapped around the copper conductor to form a shielding layer; polyvinyl chloride is extruded outside the shielding layer to form an insulating layer; the sheath material prepared in Example 2 is extruded outside the insulating layer to form a sheath layer; finally, 60 μm of the epoxy resin coating prepared in Example 3 is evenly coated on the outside of the sheath layer to form an anti-corrosion layer, thereby obtaining a corrosion-resistant power cable.
[0066] Example 6
[0067] A corrosion-resistant power cable comprises an anti-corrosion layer, a sheath layer arranged in the anti-corrosion layer, an insulating layer arranged in the sheath layer, a shielding layer arranged in the insulating layer, and a conductor arranged in the shielding layer; the conductor is a copper conductor, the shielding layer is an aluminum-plastic composite tape shielding layer, the insulating layer is polyvinyl chloride, the sheath layer is prepared by the sheath material prepared in Example 3, and the anti-corrosion layer is coated with the epoxy resin coating prepared in Example 3, specifically comprising the following steps:
[0068] An aluminum-plastic composite tape is wrapped around the copper conductor to form a shielding layer; polyvinyl chloride is extruded outside the shielding layer to form an insulating layer; the sheath material prepared in Example 3 is extruded outside the insulating layer to form a sheath layer; finally, 70 μm of the epoxy resin coating prepared in Example 3 is evenly coated on the outside of the sheath layer to form an anti-corrosion layer, thereby obtaining a corrosion-resistant power cable.
[0069] Comparative Example 1
[0070] This comparative example is a power cable, which is different from Example 6 in that the preparation method of the sheath material used is as follows, and the rest is the same.
[0071] The sheath material is prepared by the following steps:
[0072] The raw materials were weighed according to weight, and 60 parts of polyvinyl chloride, 30 parts of silicone rubber, 15 parts of ACR toughener, 5 parts of N, N′-phenylene bismaleimide, 2 parts of vulcanization accelerator NA-22, 4 parts of zinc stearate, 8 parts of diethyl phthalate, 10 parts of MXene nanosheets and 1 part of antioxidant 1010 were added into a double-roll plasticizer and mixed at 140°C for 30 minutes. The mixed rubber was then placed on a flat vulcanizer, the temperature was set to 220°C, preheated for 30 minutes, and then pressurized and vulcanized at 10 MPa for 5 minutes. After cooling, the sheath material was obtained.
[0073] Comparative Example 2
[0074] This comparative example is a power cable, which differs from Example 6 in that no anti-corrosion layer is provided, and the rest are the same.
[0075] The power cables prepared in Examples 4-6 and Comparative Examples 1-2 were subjected to performance tests: flame retardant performance test: oxygen index was measured according to the method of GB / T 2406.2-2009 "Determination of Combustion Behavior by Oxygen Index Method for Plastics"; corrosion resistance test: power cable samples were immersed in 25wt% hydrochloric acid solution, 25wt% sodium hydroxide solution, 25wt% sodium chloride solution and aqueous solution under the same conditions for 200h, and then taken out to observe surface corrosion. The test results are shown in the following table:
[0076]
[0077] It can be seen from the above table that the power cable prepared by the present invention is immersed in 25wt% hydrochloric acid solution, 25wt% sodium hydroxide solution, 25wt% sodium chloride solution and water for 200h respectively, and there is no corrosion on the surface, indicating that the power cable has excellent corrosion resistance; the limiting oxygen index is in the range of 34.6%-35.9%, indicating that the cable also has excellent flame retardant properties.
[0078] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A corrosion-resistant power cable, characterized in that: It includes an anti-corrosion layer, a sheath layer inside the anti-corrosion layer, an insulating layer inside the sheath layer, a shielding layer inside the insulating layer, and a conductor inside the shielding layer; The conductor is a copper conductor, the shielding layer is an aluminum-plastic composite tape shielding layer, the insulating layer is polyvinyl chloride, the sheath layer is made of sheath material, and the anti-corrosion layer is coated with epoxy resin paint; The sheath material is prepared by the following steps: Step A1, stirring and mixing boron nitride nanotubes and tris(hydroxymethyl)aminomethane) in a mixture of ethanol, methanol and deionized water, recorded as solution A; then dispersing dopamine hydrochloride in deionized water, recorded as solution B; then pouring solution B into solution A for ultrasonic dispersion for 10-20 minutes, and reacting for 8-12 hours under stirring conditions, after the reaction is completed, centrifuging, washing, and vacuum drying at 70°C for 10 hours to obtain BNNTs@PDA nanomaterials; Step A2, ultrasonically disperse the MXene nanosheets after HCl-LiF etching in deionized water for 30 minutes, centrifuge to obtain the supernatant, add citric acid and polyethylene glycol to the supernatant and stir to mix evenly, transfer the resulting mixed solution to a reactor, react at 160-180°C for 3-5 hours, after the reaction is completed, cool to room temperature, centrifuge, wash, redisperse the precipitate in 10 mL of deionized water, add thioglycolic acid with a pH of 7, stir to react for 20-40 minutes, centrifuge, wash, and dry to obtain MPA-C QDs / MXene nanomaterials; Step A3, dispersing BNNTs@PDA nanomaterials in deionized water, adjusting the pH to 6-6.5, adding MPA-CQDs / MXene nanomaterials, and oscillating for 12 hours using a constant temperature oscillator. After the reaction is completed, centrifuging, washing, and freeze-drying to obtain a modified filler; Step A4, weigh the raw materials by weight, add 40-60 parts of polyvinyl chloride, 20-30 parts of silicone rubber, 10-15 parts of ACR toughener, 3-5 parts of vulcanizer, 1-2 parts of vulcanization accelerator, 2-4 parts of lubricant, 5-8 parts of diethyl phthalate, 5-10 parts of modified filler and 0.5-1 part of antioxidant into a double-roll plasticizer, and mix at 120-140° C. for 30 minutes, then place the mixed rubber on a flat vulcanizer, set the temperature to 200-220° C., preheat for 30 minutes, then press vulcanize at 10 MPa for 3-5 minutes, cool, and obtain the sheath material.
2. A corrosion-resistant power cable according to claim 1, characterized in that: In step A1, the amount ratio of boron nitride nanotubes, tris(hydroxymethyl)aminomethane, ethanol, methanol and deionized water in solution A is 0.2-0.4 g: 0.15-0.45 g: 50 mL: 50 mL: 100 mL; the amount ratio of dopamine hydrochloride and deionized water in solution B is 0.8-2.0 g: 100 mL.
3. A corrosion-resistant power cable according to claim 1, characterized in that: In step A2, the dosage ratio of MXene nanosheets, citric acid, polyethylene glycol, deionized water and thioglycolic acid is 0.1-0.5 g: 2-3 g: 10 mL: 20 mL: 0.5-3 mL.
4. A corrosion-resistant power cable according to claim 1, characterized in that: In step A2, 4 mol / L sodium hydroxide solution is used to adjust the pH of thioglycolic acid.
5. The corrosion-resistant power cable according to claim 1, characterized in that: In step A3, the dosage ratio of BNNTs@PDA nanomaterial, MPA-C QDs / MXene nanomaterial and deionized water is 0.5-1 g: 0.2-0.4 g: 20 mL.
6. The corrosion-resistant power cable according to claim 1, characterized in that: The epoxy resin coating is prepared by the following steps: Step B1, add perfluorohexylethyl acrylate and 5-hexenylmethyldichlorosilane into a flask and mix evenly, then add dibenzoyl peroxide and diethylene glycol dimethyl ether, then introduce nitrogen into the system, and heat the system to 80-95° C. to react for 6-8 hours. After the reaction is completed, cool to 60° C., then add butyl acetate and deionized water, wash and separate, and then dry the precipitate at 60° C. for 5 hours to obtain a fluorine-containing resin; Step B2, add epoxy resin E51 and butyl acetate into a flask, heat to 50°C and stir for 30 minutes, then add fluorine-containing resin, dibutyltin dilaurate and triethylamine in sequence, continue stirring and react for 6-8 hours, after the reaction is completed, centrifuge, wash 3-5 times, and then distill under reduced pressure to obtain a modified epoxy resin; Step B3, weigh the raw materials by weight, add 30-40 parts of modified epoxy resin and 7-10 parts of ceramic powder into a ball mill and ball mill at a speed of 300-400rpm for 1-2h, then add 0.1-0.3 parts of defoaming agent and 15-25 parts of deionized water in a high-speed rotary machine and stir at a speed of 800-1000rpm for 20min, finally add 0.2-0.5 parts of leveling agent, 1-5 parts of curing agent, 0.5-0.8 parts of antistatic agent and 0.1-0.3 parts of thickener and continue stirring for 30min to obtain epoxy resin coating.
7. A corrosion-resistant power cable according to claim 6, characterized in that: In step B1, the usage ratio of perfluorohexylethyl acrylate, 5-hexenyltrimethoxysilane, dibenzoyl peroxide, diethylene glycol dimethyl ether, butyl acetate and deionized water is 1-3 g: 2-3 g: 0.05 g: 4-6 mL: 5 mL: 15 mL.
8. The corrosion-resistant power cable according to claim 6, characterized in that: In step B2, the usage ratio of epoxy resin E51, butyl acetate, fluorine-containing resin, dibutyltin dilaurate and triethylamine is 30-40 g: 15-20 mL: 1.5-3.5 g: 0.2-0.3 g: 10 g.
9. The method for preparing a corrosion-resistant power cable according to claim 1, characterized in that: The following steps are involved: Wrap an aluminum-plastic composite tape around the copper conductor to form a shielding layer; then extrude polyvinyl chloride outside the shielding layer to form an insulating layer; then extrude the sheath material outside the insulating layer to form a sheath layer; finally, evenly apply 50-70μm epoxy resin paint on the outside of the sheath layer to form an anti-corrosion layer, thereby obtaining a corrosion-resistant power cable.