Method and system for optimizing process parameters for suppressing porosity in high-power laser shaping welding

By optimizing the adjustable ring laser beam diameter and center point line energy and controlling welding process parameters, the problem of pore defects in high-power laser welding is solved, and the stability and quality improvement of the welding process is achieved. It is suitable for aluminum alloy medium and thick wall components welding.

CN118162740BActive Publication Date: 2024-11-19HUAZHONG UNIV OF SCI & TECH +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410299181.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2024-11-19
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

During high-power laser welding, especially when welding highly thermally conductive materials such as aluminum alloys, pore defects are prominent, and the energy distribution regulation of traditional Gaussian beams is limited, resulting in unstable welding, and the existing technology lacks a systematic pore improvement solution.

Method used

By obtaining the relationship between the adjustable ring laser beam diameter and the center point line energy and welding process parameters, optimize the process parameters such as laser power, welding speed and point-ring laser power ratio, control the melting depth to beam diameter ratio and center Pointed and line energy achieves precise control of laser energy distribution.

Benefits of technology

It significantly reduces pore defects, improves welding quality and efficiency, and provides a systematic pore improvement solution, suitable for welding different types of aluminum alloy medium-thick wall components, simplifying the process design cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118162740B_ABST
    Figure CN118162740B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of high-power laser welding, and discloses a method and system for optimizing process parameters for suppressing pores in high-power laser shaping welding, obtaining the relationship between the diameter of an adjustable ring laser beam and the center point line energy and welding process parameters; establishing the optimization constraint conditions of the diameter of an adjustable ring laser beam and the center point line energy; obtaining the preset range of process parameters; substituting the process parameter values ​​within the preset range into the optimization constraint conditions of the diameter of an adjustable ring laser beam and the center point line energy, and then the process parameter combination that simultaneously satisfies the optimization constraint conditions of the diameter of an adjustable ring laser beam and the center point line energy is the optimized process parameter. The present invention flexibly adjusts the power ratio of the center point Gaussian beam and the outer ring annular beam, and on the premise of ensuring a large penetration depth, significantly improves the pore problem caused by high-speed laser welding of aluminum alloys, and can provide a reference for high-quality welding of aluminum alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-power laser welding, and in particular relates to a method and system for optimizing process parameters for pore suppression in high-power laser shaping welding. Background Art

[0002] At present, aluminum alloy medium and thick wall components have the advantages of low density and high specific strength, and have been widely used in rail transportation, aerospace and other fields. High-power laser welding technology has the characteristics of high energy density, low heat input and good flexibility, which provides an effective means for the efficient welding of aluminum alloy medium and thick wall components. However, there are still prominent problems of porosity defects in the welding process, which are mostly caused by the collapse of the keyhole during laser deep fusion welding. In recent years, laser beam shaping technology has been used in the context of engineering light-matter interaction to solve the shortcomings of using focused Gaussian beams in laser manufacturing of metals. Among them, adjustable ring lasers have received widespread attention. The core idea of ​​adjustable ring laser welding technology is to introduce a ring laser beam on the basis of high-power (Gaussian spot) laser welding to regulate the spatial distribution of laser energy. Studies have shown that compared with Gaussian beams, the use of adjustable ring lasers can improve the stability of the laser welding process within a wider range of process parameters. However, due to the relatively new nature of this type of laser, the research foundation for its application in the field of welding is weak, and there are few reports on improving porosity, and no systematic porosity improvement plan has been formed.

[0003] Through the above analysis, the problems and defects of the prior art are as follows:

[0004] (1) During high-power laser welding, especially when welding high-thermal-conductivity and high-reflectivity metals such as aluminum alloys, the problem of pore defects is particularly prominent. These pores are mostly caused by the collapse of the keyhole during laser deep-melting welding.

[0005] (2) Traditional Gaussian beams have limitations in regulating energy distribution. During Gaussian laser welding, the energy is mainly concentrated in the center of the beam, resulting in a large thermal gradient, which can easily cause instability in the welding process and lead to frequent keyhole collapse.

[0006] (3) The existing technology of shaping laser beam is relatively new, and the research foundation for its application in the field of welding is weak. There are few reports on improving porosity, and no systematic porosity improvement plan has been formed. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a method and system for optimizing process parameters for pore suppression in high-power laser shaping welding.

[0008] The present invention is achieved by a method for optimizing process parameters for suppressing pores in high-power laser shaping welding, comprising:

[0009] The first step is to obtain the relationship between the adjustable annular laser beam diameter and the center point line energy and the welding process parameters;

[0010] The second step is to establish the optimization constraint conditions of the adjustable annular laser beam diameter and the center point line energy; and obtain the preset range of the process parameters;

[0011] In the third step, the process parameter values ​​within the preset range are substituted into the optimization constraints of the adjustable annular laser beam diameter and the center point line energy. The process parameter combination that satisfies the optimization constraints of the adjustable annular laser beam diameter and the center point line energy is the optimized process parameter.

[0012] Furthermore, the process parameters include laser power, welding speed, and spot-ring laser power ratio.

[0013] Furthermore, the relationship between the adjustable annular laser beam diameter and the welding process parameters is obtained by referring to the IS0 11146-1:2021 (en) standard. For any spot laser beam, D4σ is defined as the beam diameter. The calculation method is to use the laser beam intensity information to solve the second-order moment of the intensity distribution function. The detailed calculation steps are as follows:

[0014] By setting the central Gaussian beam intensity E c (x, y) and the outer ring beam intensity E r (x, y) are added to obtain the light intensity distribution E(x, y) of the entire adjustable annular beam.

[0015] E(x,y)=E c (x,y)+E r (x,y)

[0016] The center coordinate of the beam (x c ,y c ) can be calculated as follows:

[0017]

[0018]

[0019] Represents the normalized weighted integral of the power density distribution, calculated as follows:

[0020]

[0021]

[0022] For a Gaussian beam with radius w and center at (0,0), the formula is as follows:

[0023]

[0024] Therefore, the beam radius adopted by IS011146-1:2021(en) is defined as:

[0025] w=2σ x

[0026] The beam diameter D4σ is twice the beam radius mentioned above, and is expressed as follows:

[0027] D4σ=2w

[0028] Further, the steps of obtaining the center point line energy and welding process parameters are as follows:

[0029] Get the center point line energy. The expression of the center point line energy q is:

[0030]

[0031] Among them, P c is the laser power of the central point light source, and v is the welding speed.

[0032] The optimization constraint condition of the ratio of the penetration depth to the beam diameter is:

[0033]

[0034] Where h is the preset target melting depth, M col represents the collimation coefficient, M focus represents the focus imaging ratio;

[0035] Furthermore, the optimization constraint of the beam diameter D4σ is:

[0036]

[0037] The optimization constraints of the center point line energy are:

[0038] q min <q<q max

[0039] Among them, q min and q max are the maximum and minimum center point line energies under empirical conditions.

[0040] Furthermore, the method for optimizing process parameters for suppressing pores in high-power laser shaping welding obtains a preset range of the process parameters according to the working range of each parameter of the welding system or the process requirements;

[0041] The process parameter values ​​are input into the optimization constraints. When the process parameters simultaneously meet the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, they are retained. Otherwise, they are discarded and the next set of process parameters are verified.

[0042] Another object of the present invention is to provide a computer device, comprising a memory and a processor, wherein the memory stores a computer program, and when the computer program is executed by the processor, the processor executes the method for optimizing process parameters for pore suppression in high-power laser shaping welding.

[0043] Another object of the present invention is to provide a computer-readable storage medium storing a computer program, which, when executed by a processor, enables the processor to execute the method for optimizing process parameters for pore suppression in high-power laser shaping welding.

[0044] Another object of the present invention is to provide an information data processing terminal, which is used to implement the method for optimizing process parameters for pore suppression in high-power laser shaping welding.

[0045] Another object of the present invention is to provide a high-power laser shaping welding pore suppression process parameter optimization system based on the high-power laser shaping welding pore suppression process parameter optimization method, the high-power laser shaping welding pore suppression process parameter optimization system comprises:

[0046] A parameter acquisition module is used to obtain the relationship between the adjustable annular laser beam diameter and the center point line energy and the welding process parameters;

[0047] A condition establishment module is used to establish the optimization constraint conditions of the adjustable annular laser beam diameter and the center point line energy; and to obtain the preset range of the process parameters;

[0048] The condition optimization module is used to substitute the process parameter values ​​within a preset range into the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, and the process parameter combination that simultaneously satisfies the optimization constraints of the adjustable annular laser beam diameter and the center point line energy is the optimized process parameter.

[0049] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:

[0050] First, the present invention proposes an aluminum alloy laser welding process based on an adjustable ring laser. It does not require complicated external tooling. By flexibly adjusting the power ratio of the center point Gaussian beam and the outer ring annular beam, it significantly improves the porosity problem caused by high-speed laser welding of aluminum alloys while ensuring a large melting depth. This can provide a reference for high-quality welding of aluminum alloys.

[0051] Second, the present invention starts from the stability of the small hole, takes the ratio of penetration depth to beam diameter as an indicator to characterize the porosity, takes the linear energy of the center point of the weld as an evaluation indicator of penetration depth, and establishes a correlation between the ratio of penetration depth to beam diameter and the linear energy of the center point and the process parameters to be optimized. By controlling the constraints of the ratio of penetration depth to beam diameter and the linear energy of the center point, the constraints on the process parameters are realized, and then multiple groups of better process parameters are obtained, which can be directly used in engineering applications, to achieve precise control of the beam diameter and the spatial energy distribution of the beam, inhibit the generation of pores during welding, and finally achieve welding with fewer pores.

[0052] The present invention can accurately control the central energy distribution of the laser beam during the welding process, and can predict the penetration depth of the weld joint to obtain the penetration depth that meets the application requirements. Adjustable annular laser welding is different from single laser welding. The addition of annular beam can achieve the effect of expanding the opening area of ​​the welding hole, thereby reducing the bubbles formed by the closing and collapse of the hole during deep penetration welding, while expanding the molten pool and extending the solidification time of the molten pool, providing more time for the bubbles to escape, thereby reducing the bubbles solidifying in the weld to form pores.

[0053] The present invention does not require a large number of process tests to obtain process parameters with less pores and greater penetration depth. Only the weld penetration result is required to optimize the process parameters using the method of the present invention. The operation is simple and the process design cycle is significantly shortened.

[0054] The technical solution of the present invention includes a systematic solution for improving porosity in the high-power laser welding process, which can effectively improve the prominent problem of porosity defects faced by medium- and thick-walled components of aluminum alloys for a long time while ensuring a large melting depth, filling the research gap in improving porosity in high-power laser shaping welding.

[0055] Thirdly, the advantages and positive technical effects of the present invention are also reflected in:

[0056] Significant pore suppression effect: The present invention significantly reduces pore defects in the aluminum alloy welding process by optimizing process parameters, thereby improving the quality and reliability of the welded joint.

[0057] Improved welding efficiency: By precisely controlling laser energy distribution and welding parameters, the present invention not only improves welding quality but also helps to improve welding efficiency.

[0058] Wide applicability: The optimized steps and standardized measurement methods of this method make it widely applicable to the welding of medium-thick wall components of different types of aluminum alloys, and it has strong practicality and universality.

[0059] Systematization of process parameter optimization: The present invention provides a systematic process parameter optimization method, which can be adjusted and optimized according to specific application requirements, providing a more flexible and efficient welding process selection. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 It is a flow chart of a method for optimizing process parameters for suppressing pores in high-power laser shaping welding provided by an embodiment of the present invention;

[0061] Figure 2 1. It is a schematic diagram of the structure of a system for optimizing process parameters for suppressing pores in high-power laser shaping welding provided by an embodiment of the present invention;

[0062] Figure 3 It is a flow chart of a method for optimizing process parameters for suppressing pores in adjustable annular laser welding provided by an embodiment of the present invention;

[0063] Figure 4 : is a relationship diagram between the laser power ratio and the beam diameter of the adjustable annular laser welding spot provided by an embodiment of the present invention;

[0064] Figure 5 is a welding defect diagram in adjustable annular laser welding provided by an embodiment of the present invention;

[0065] Figure 6 is a three-dimensional schematic diagram of energy density provided by an embodiment of the present invention;

[0066] Figure 7 is a schematic front cross-sectional view of energy density provided by an embodiment of the present invention;

[0067] Figure 8 is a top cross-sectional schematic diagram of energy density provided by an embodiment of the present invention;

[0068] Fig. 9A The schematic diagram of pure Gaussian spot laser welding process parameters after welding is shown schematically;

[0069] Fig. 9B The schematic diagram of welding under the combination of process parameters b in a common design is shown schematically;

[0070] Fig. 9C The welding schematic diagram under the optimized process parameter c combination of the present invention is schematically shown. DETAILED DESCRIPTION

[0071] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0072] The present invention mainly improves the following problems and defects of the prior art and achieves significant technical progress:

[0073] Solution to the pore defect problem: By optimizing the adjustable annular laser beam diameter and the center point line energy, the invention directly regulates the key factors of pore formation, thereby effectively inhibiting the generation of pores.

[0074] Energy distribution control: By establishing the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, the invention achieves precise control of laser energy distribution and improves the problem of uneven energy distribution in traditional Gaussian beam welding.

[0075] Improved stability of welding process: By optimizing process parameters such as laser power, welding speed and spot-to-ring laser power ratio, the present invention improves the stability of the welding process, thereby reducing welding defects.

[0076] Accurate calculation of beam diameter: The IS011146-1:2021(en) standard is used to obtain the relationship between the adjustable ring laser beam diameter and the welding process parameters, ensuring the accuracy and consistency of the beam measurement.

[0077] Two specific embodiments of the present invention are:

[0078] Example 1 - Precision welding of aluminum alloy carriages for high-speed trains

[0079] Welding parameter adjustment: First, the welding parameters (laser power, welding speed and spot-ring laser power ratio) are precisely adjusted according to the specific aluminum alloy material and structural requirements of the high-speed train carriage. This adjustment is based on the thickness, shape and expected load-bearing capacity of the aluminum alloy plate of the carriage.

[0080] Application of adjustable ring laser welding technology: Using adjustable ring laser technology, the keyhole stability of the welding process is effectively improved by precisely controlling the adjustable ring laser beam diameter and the center point line energy. This helps to reduce pores and other defects during the welding process.

[0081] Weld morphology optimization: As high-speed trains have high requirements for aerodynamic performance, the smoothness and uniformity of the welds are crucial. Adjustable circular laser welding technology can achieve more detailed and smooth welds, which is conducive to reducing wind resistance.

[0082] Quality monitoring and assessment: During the welding process, welding parameters and weld morphology are monitored in real time to ensure that the welding quality meets the safety and performance standards of high-speed trains.

[0083] Example 2 - High-precision welding of spacecraft aluminum alloy bracket

[0084] Parameter optimization in extreme environments: Considering that spacecraft operate in extreme temperature and pressure environments, welding parameters (laser power, welding speed, and spot-ring laser power ratio) need to be strictly optimized for these conditions. This includes fine-tuning the laser energy distribution and heat input to suit the characteristics of the aluminum alloy bracket.

[0085] Complex structure welding technology: Adjustable circular laser welding technology is used to process the complex seams of spacecraft aluminum alloy brackets. This technology can flexibly adapt to irregular welding paths and complex geometric structures while maintaining the uniformity and strength of the weld.

[0086] High-load welding quality assurance: To ensure that welded components can withstand high loads and strong vibrations, special attention is paid to the suppression of pores and defects during welding. This is achieved by precisely controlling welding parameters and monitoring the weld formation process in real time.

[0087] Evaluation and testing of welding effects: After welding is completed, the weld joint undergoes rigorous quality evaluation, including fatigue testing and structural integrity inspection to ensure it meets the stringent requirements of the spacecraft.

[0088] like Figure 1 As shown, the method for optimizing process parameters for suppressing pores in high-power laser shaping welding provided by an embodiment of the present invention comprises the following steps:

[0089] S101: Obtaining the relationship between the diameter of the adjustable annular laser beam and the center point line energy and the welding process parameters;

[0090] S102: establishing optimization constraints of the diameter of the adjustable annular laser beam and the center point line energy; obtaining a preset range of process parameters;

[0091] S103: Substituting the process parameter values ​​within the preset range into the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, the process parameter combination that satisfies the optimization constraints of the adjustable annular laser beam diameter and the center point line energy is the optimized process parameter.

[0092] In the embodiment of the present invention, the process parameters include laser power, welding speed, and spot-ring laser power ratio.

[0093] In the embodiment of the present invention, the relationship between the adjustable annular laser beam diameter and the welding process parameters is obtained by referring to the IS011146-1:2021(en) standard. For any spot laser beam, D4σ is defined as the beam diameter. The calculation method is to use the laser beam intensity information to solve the second-order moment of the intensity distribution function. The detailed calculation steps are as follows:

[0094] By setting the central Gaussian beam intensity E c (x, y) and the outer ring beam intensity Er (x, y) are added to obtain the light intensity distribution E(x, y) of the entire adjustable annular beam.

[0095] E(x,y)=E c (x,y)+E r (x,y)

[0096] The center coordinate of the beam (x c ,y c ) can be calculated as follows:

[0097]

[0098]

[0099] Represents the normalized weighted integral of the power density distribution, calculated as follows:

[0100]

[0101]

[0102] For a Gaussian beam with radius w and center at (0,0), the formula is as follows:

[0103]

[0104] Therefore, the beam radius adopted by IS0 11146-1:2021(en) is defined as:

[0105] w=2σ x

[0106] The beam diameter D4σ is twice the beam radius mentioned above, and is expressed as follows:

[0107] D4σ=2w

[0108] In the embodiment of the present invention, the steps of obtaining the center point line energy and welding process parameters are as follows:

[0109] Get the center point line energy. The expression of the center point line energy q is:

[0110]

[0111] Among them, P c is the laser power of the central point light source, and v is the welding speed.

[0112] Furthermore, the optimization constraint of the beam diameter D4σ is:

[0113]

[0114] Where h is the preset target melting depth, M col represents the collimation coefficient, M focus represents the focus imaging ratio;

[0115] The optimization constraints of the center point line energy are:

[0116] q min <q<q max

[0117] Among them, q min and q max are the maximum and minimum center point line energies under empirical conditions.

[0118] In an embodiment of the present invention, the preset range of the process parameters is obtained according to the working range of each parameter of the welding system or the process requirements.

[0119] In an embodiment of the present invention, the process parameter value is input into the optimization constraint condition, and when the process parameter value satisfies the optimization constraint conditions of the adjustable annular laser beam diameter and the center point line energy at the same time, it is retained; otherwise, it is discarded and the next set of process parameters is verified.

[0120] like Figure 2 As shown, the process parameter optimization system for suppressing pores in high-power laser shaping welding provided by the embodiment of the present invention includes:

[0121] A parameter acquisition module is used to obtain the relationship between the adjustable annular laser beam diameter and the center point line energy and the welding process parameters;

[0122] A condition establishment module is used to establish the optimization constraint conditions of the adjustable annular laser beam diameter and the center point line energy; and to obtain the preset range of the process parameters;

[0123] The condition optimization module is used to substitute the process parameter values ​​within a preset range into the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, and the process parameter combination that simultaneously satisfies the optimization constraints of the adjustable annular laser beam diameter and the center point line energy is the optimized process parameter.

[0124] Porosity is one of the main defects that occur during high-power laser welding, and is particularly prominent in the welding of aluminum alloy medium and thick plates. The following is a detailed introduction to the method of the present invention using the welding of aluminum alloy medium and thick plates as an example. High-power adjustable ring laser welding technology provides an effective means for suppressing pores in the welding process of aluminum alloy medium and thick plates. However, high-power adjustable ring laser welding technology changes the spatial energy distribution of the beam, the energy coupling mechanism of the point and ring lasers is unclear, and the selection of process parameters is very blind, which is prone to the following problems: Figure 5The present invention proposes a method for accurately controlling the laser beam diameter and the beam spatial energy distribution to achieve welding process optimization with large weld penetration and small porosity, such as Figure 1 and Figure 3 As shown, the method of the present invention includes the following steps S1 to S4.

[0125] S1, obtain the relationship between the adjustable annular laser beam diameter and the center point line energy and welding process parameters.

[0126] The process parameters in the present invention are mainly laser power, welding speed, and spot-ring laser power ratio.

[0127] Preferably, the step of obtaining the relationship between the adjustable annular laser beam diameter and the welding process parameters is:

[0128] In this implementation case, the CFX-8kW programmable spot fiber laser from nLIGHT Laser Company is used. The power of the center spot laser and the ring laser are adjusted in a certain ratio. For example, when the laser power ratio of the center beam to the ring beam (P c / P r )=6:4, that is, the center power P c Accounting for 60% of the total power, the ring power P r It accounts for 40% of the total power.

[0129] In this implementation case, the equivalent beam diameter under different point ring laser ratios is as follows: Figure 4 shown.

[0130] The line energy q at the center of the weld is used as an evaluation index for the depth of penetration. Figure 6 , Figure 7 , Figure 8 As shown in the figure, since the annular energy mainly acts on both sides of the weld, and the keyhole depth is mainly maintained by the steam pressure, the linear energy at the center of the weld is selected to evaluate the weld penetration. The linear energy q at the center of the weld is shown as follows:

[0131]

[0132] Among them, P c is the laser power of the central point light source, and v is the welding speed.

[0133] S2, establishing optimization constraints of the adjustable annular laser beam diameter and center point line energy;

[0134] Determine the minimum length of the adjustable annular laser beam diameter D4σ. According to the long liquid column stability theory, the relative stability of the small hole can be achieved when the circumference of the small hole is greater than the depth of the small hole. In addition, the diameter of the steam capillary in laser beam welding is in a certain proportional relationship with the diameter of the laser spot on the surface of the irradiated material.

[0135] According to experimental statistics, the optimization constraint condition of the ratio of melting depth to beam diameter is:

[0136]

[0137] Where h is the preset target melting depth, M col represents the collimation coefficient, M focus represents the focusing imaging ratio; that is, the optimization constraint condition of the adjustable annular laser beam diameter is:

[0138]

[0139] Among them, in this implementation case, M col =1.75,M focus =1.5; the optimization constraint condition of the center point line energy is:

[0140] q min <q<q max

[0141] Among them, q min and q max are the maximum and minimum center point line energies under empirical conditions.

[0142] S3, obtaining a preset range of the process parameter.

[0143] Obtain the energy ratio threshold under the target penetration depth. Assume that the target penetration depth of the test is 4.0-4.6 mm. According to the above constraints, D4σ in this embodiment needs to be greater than 0.27 mm. Figure 4 The relationship diagram between the beam diameter and the spot-ring laser power ratio provided shows that the critical range of the spot-ring laser power ratio in this embodiment is 6:4, that is, the ring ratio shall not be less than 40%;

[0144] Obtain the center point line energy range under the target penetration depth. Since the center point line energy and weld penetration depth are basically linearly related, the correlation can be established based on several sets of experimental results. Therefore, the line energy range can better ensure that the experimental results of the designed process parameters are near the target penetration depth.

[0145] Specifically, the range of process parameters can be roughly selected according to the reachable range of the welding equipment or the range required in the actual operation process. In this way, the variation range of the point laser power can be roughly obtained as [P Cmin , P Cmax ], welding speed variation range is [v min , v max ], the range of the power ratio of the spot ring laser is [R min , R max ].

[0146] The points in the above variation interval are gradually substituted into the above optimization constraints by interpolation. The parameter combination that satisfies all the above constraints is retained. Otherwise, this group of parameters is discarded and the verification calculation of the next group of parameters is performed. In this way, a better process parameter combination corresponding to the target melting depth can be screened out from the above rough selection range, and the optimal process parameters can be directly selected next time it is used. It is simple and convenient.

[0147] A set of parameters for pure Gaussian spot laser welding experimental design was randomly selected, for example, parameter a: total power of 3500W, welding speed of 40mm / s, and spot-ring laser power ratio of 10:0. A set of parameters for a common experimental design was randomly selected, parameter b: total power of 4290W, welding speed of 40mm / s, and spot-ring laser power ratio of 7:3; a set of optimized experimental design parameters was selected according to this patent application, parameter c: total power of 6000W, welding speed of 60mm / s, and spot-ring laser power ratio of 5:5. Welding tests were carried out respectively, and the longitudinal cross-section morphology of the weld was as follows Figures 9A to 9C The experimental results show that the porosity of the welds optimized by the process parameters of this method is significantly lower than that of the process parameters of the ordinary experimental design at similar penetration depth.

[0148] The above method steps only list the process of designing the corresponding process parameters for achieving 6061 aluminum alloy welding with a specified melting depth and few pores. In fact, the method of the present invention is also applicable to process design under other materials, such as when the welding base material is steel; the method of the present invention is also applicable to welding under other laser shaping conditions, such as Bessel beam laser welding.

[0149] In summary, the present invention starts from ensuring the stability of the small holes during the welding process, takes the ratio of penetration depth to beam diameter as the porosity evaluation index, takes the linear energy at the center of the weld as the penetration evaluation index, and establishes a relationship between the adjustable annular laser beam diameter and the center point linear energy and the process parameters to be optimized. By controlling the constraints of the adjustable annular laser beam diameter and the center point linear energy, the constraints of the process parameters are realized, and then multiple groups of better process parameters are obtained, which can be directly used in engineering applications, to achieve precise control of the beam diameter and spatial distribution, inhibit the generation of pores during welding, and finally achieve welding with fewer pores, which significantly improves the welding quality and efficiency.

[0150] It should be noted that the embodiments of the present invention can be implemented by hardware, software, or a combination of software and hardware. The hardware part can be implemented using dedicated logic; the software part can be stored in a memory and executed by an appropriate instruction execution system, such as a microprocessor or dedicated design hardware. It can be understood by a person of ordinary skill in the art that the above-mentioned devices and methods can be implemented using computer executable instructions and / or contained in a processor control code, such as a carrier medium such as a disk, CD or DVD-ROM, a programmable memory such as a read-only memory (firmware), or a data carrier such as an optical or electronic signal carrier. Such code is provided on the carrier medium. The device and its modules of the present invention can be implemented by hardware circuits such as very large-scale integrated circuits or gate arrays, semiconductors such as logic chips, transistors, etc., or programmable hardware devices such as field programmable gate arrays, programmable logic devices, etc., can also be implemented by software executed by various types of processors, and can also be implemented by a combination of the above-mentioned hardware circuits and software, such as firmware.

[0151] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for optimizing process parameters for pore suppression in high-power laser shaping welding, characterized in that: include: The first step is to obtain the relationship between the adjustable annular laser beam diameter and the center point line energy and the welding process parameters; The second step is to establish the optimization constraint conditions of the adjustable annular laser beam diameter and the center point line energy; and obtain the preset range of the process parameters; The third step is to substitute the process parameter values ​​within the preset range into the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, and then the process parameter combination that satisfies the optimization constraints of the adjustable annular laser beam diameter and the center point line energy is the optimized process parameter; The relationship between the adjustable annular laser beam diameter and welding process parameters is obtained by referring to the IS011146-1:2021(en) standard. For any spot laser beam, D4σ is defined as the beam diameter. The calculation method is to use the laser beam intensity information to solve the second-order moment of the intensity distribution function. The detailed calculation steps are as follows: By setting the central Gaussian beam intensity E c (x, y) and the outer ring beam intensity E r (x, y) are added to obtain the light intensity distribution E(x, y) of the entire adjustable annular beam: E(x,y)=E c (x,y)+E r (x,y) The center coordinate of the beam (x c ,y c ) can be calculated as follows: Represents the normalized weighted integral of the power density distribution, calculated as follows: For a Gaussian beam with radius w and center at (0,0), the formula is as follows: Therefore, the beam radius adopted by IS011146-1:2021(en) is defined as: in=2σ x The beam diameter D4σ is twice the beam radius mentioned above, and is expressed as follows: D4σ=2w; The steps to obtain the center point line energy and welding process parameters are: Get the center point line energy. The expression of the center point line energy q is: Among them, P c is the laser power of the central point light source, v is the welding speed; The optimization constraint of beam diameter D4σ is: Where h is the preset target melting depth, M col represents the collimation coefficient, M focus represents the focus imaging ratio; The optimization constraints of the center point line energy are: q min <q<q max Among them, q min and q max are the maximum and minimum center point line energies under empirical conditions.

2. The method for optimizing process parameters for suppressing pores in high-power laser shaping welding according to claim 1, characterized in that: The process parameters include laser power, welding speed, and spot-ring laser power ratio.

3. The method for optimizing process parameters for pore suppression in high-power laser shaping welding according to claim 1, characterized in that: The method for optimizing process parameters for pore suppression in high-power laser shaping welding obtains a preset range of the process parameters according to the working range of each parameter of the welding system or the process requirements; The process parameter values ​​are input into the optimization constraints. When the process parameter values ​​simultaneously meet the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, they are retained. Otherwise, they are discarded and the next set of process parameters are verified.

4. A computer device, characterized in that: The computer device includes a memory and a processor, the memory stores a computer program, and when the computer program is executed by the processor, the processor executes the method for optimizing process parameters for pore suppression in high-power laser shaping welding as described in any one of claims 1 to 3.

5. A computer-readable storage medium storing a computer program, wherein when the computer program is executed by a processor, the processor executes the method for optimizing process parameters for pore suppression in high-power laser shaping welding as claimed in any one of claims 1 to 3.

6. An information data processing terminal, characterized in that: The information data processing terminal is used to implement the method for optimizing process parameters for pore suppression in high-power laser shaping welding as described in any one of claims 1 to 3.

7. A system for optimizing process parameters for suppressing pores in high-power laser shaping welding based on the method for optimizing process parameters for suppressing pores in high-power laser shaping welding according to any one of claims 1 to 3, characterized in that: The high-power laser shaping welding process parameter optimization system for suppressing pores includes: A parameter acquisition module is used to obtain the relationship between the adjustable annular laser beam diameter and the center point line energy and the welding process parameters; A condition establishment module is used to establish the optimization constraint conditions of the adjustable annular laser beam diameter and the center point line energy; and to obtain the preset range of the process parameters; The condition optimization module is used to substitute the process parameter values ​​within a preset range into the optimization constraints of the adjustable annular laser beam diameter and the center point line energy, and the process parameter combination that simultaneously satisfies the optimization constraints of the adjustable annular laser beam diameter and the center point line energy is the optimized process parameter.

Citation Information

Patent Citations

  • Process parameter optimization method and system for pore suppression in laser stirring welding

    CN113305435A

  • High-end decorative stainless steel sheet T-shaped joint laser welding process parameter optimization method

    CN113857675A

  • Axial point ring multi-focus laser welding method

    CN116423041A

  • Laser beam welding method

    JP2010167428A

  • Device and Method for Laser Processing

    US20100206857A1