A method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as raw material

The chemical vapor deposition method uses MTS as raw material to grow silicon carbide whiskers on silicon carbide fibers, which solves the problems of long preparation cycle, high cost and poor performance in the prior art, and achieves high purity and high efficiency silicon carbide whiskers Preparation, suitable for reinforced toughening applications of ceramic or metal-based composites.

CN118186587BActive Publication Date: 2024-11-19HUNAN CARBON SOURCE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410514553.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-11-19
Estimated Expiration
2044-04-26

AI Technical Summary

Technical Problem

The existing silicon carbide whisker preparation methods have problems such as long preparation cycle, high reaction temperature, many impurities and high cost, resulting in poor performance.

Method used

Using chemical vapor deposition method, using methyl trichlorosilane (MTS) as raw material, combined with argon and hydrogen, through specific temperature and flow control, silicon carbide whiskers are directly grown on silicon carbide fibers, simplifying the process flow and reducing costs .

Benefits of technology

It realizes the high-purity preparation of silicon carbide whiskers, simplifies the process flow, shortens the preparation cycle, reduces costs, and improves the performance and application prospects of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118186587B_ABST
    Figure CN118186587B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material, wherein silicon carbide fiber is used as a matrix and is obtained by chemical vapor deposition. The present invention controls the purity of the raw material methyltrichlorosilane MTS, as well as the mixed gas flow ratio and temperature of chemical vapor deposition. Compared with the general CVD method, the process is simpler, the process is easy to control, and the silicon carbide whiskers finally obtained have high purity. The silicon carbide whiskers obtained by the present invention can be used for the reinforcement and toughening of ceramic-based or metal-based composite materials, and have good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor materials, and in particular to a method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material. Background Art

[0002] Silicon carbide is the third generation of wide bandgap semiconductor materials after the first generation of elemental semiconductors and the second generation of compound semiconductors. It has the characteristics of wide bandgap, high thermal conductivity, and high critical breakdown electric field, and is particularly suitable for the production of electronic devices in harsh working environments such as high temperature and strong radiation. In addition, its one-dimensional and quasi-one-dimensional materials also have great application potential in optoelectronics, field emission devices, and micro-mechanics. Therefore, SiC nanowires have important research value.

[0003] Silicon carbide ceramics have excellent comprehensive properties such as high strength, high thermal conductivity, high electrical conductivity, high hardness, creep resistance, wear resistance, corrosion resistance, oxidation resistance and thermal stability. When it exists in the form of whiskers, there are two crystal forms: α-type and β-type. Among them, β-type silicon carbide whiskers are the products with the highest hardness, maximum modulus, maximum tensile strength and strongest heat resistance among the currently known whiskers. They have a high cost-effectiveness and are easy to compound with materials.

[0004] The strength, hardness, toughness and high temperature heat resistance of materials reinforced and toughened by SiC whiskers are greatly improved. As an efficient reinforcing material, silicon carbide whiskers can prevent the further expansion of microcracks through crack deflection, crystal breaking, whisker pull-out effect and crack bridging, thereby strengthening and toughening composite materials. Compared with similar fibers, SiC whiskers have higher tensile and tensile moduli, and have the advantages of low cost and easy processing, making them the most suitable reinforcement and toughening body for metal-based composites and ceramic-based composites among silicon carbide materials.

[0005] The existing methods for preparing silicon carbide whiskers include gas phase carbon source method, solid phase carbon source method and liquid phase carbon source method. They have the following disadvantages:

[0006] 1. The preparation cycle is long, taking 1-7 days;

[0007] 2. The reaction temperature is high and there are many whisker impurities;

[0008] 3. It needs to be carried out in stages, and a suitable substrate must be synthesized before the whiskers are deposited, which is costly. Summary of the invention

[0009] The present invention aims to provide a method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material, so as to solve the technical problems that the existing silicon carbide whisker preparation method is complicated and the product performance is poor.

[0010] To achieve the above object, the present invention provides a method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material, wherein silicon carbide fibers are used as a matrix and chemical vapor deposition is performed to obtain silicon carbide whiskers; wherein a mixed gas of argon, hydrogen and methyltrichlorosilane (MTS) is introduced into the chemical vapor deposition, and the flow rates of the three are 3-6 L / min, 6-12 L / min and 1-2 L / min, respectively; and the temperature of the chemical vapor deposition is controlled as follows:

[0011] (A) uniformly heating from room temperature to 600°C over 1.5 to 2 hours and keeping the temperature for 1 to 2 hours;

[0012] (B) Continue to raise the temperature to 950-1200° C. over 2-3 hours and keep it at that temperature for 2 hours;

[0013] (C) Deposition at 950-1200°C for 2-4 hours.

[0014] Preferably, the flow rates of argon, hydrogen and methyltrichlorosilane MTS are 3 L / min, 6 L / min and 1 L / min respectively.

[0015] Preferably, the purity of the MTS is 4N.

[0016] Preferably, the temperature of chemical vapor deposition is controlled as follows:

[0017] (A) The temperature is raised uniformly from room temperature to 600°C over 1.5 hours and kept at this temperature for 1 hour;

[0018] (B) Continue to raise the temperature to 1100°C over 2 hours and keep it at that temperature for 2 hours;

[0019] (C) Deposition at 1100°C for 4 hours.

[0020] Preferably, chemical vapor deposition is performed using a CVD deposition furnace, the furnace chamber is cleaned, the silicon carbide fiber is regularly wound on the tooling of the graphite material table, the furnace door is closed, and the vacuum is drawn to measure the pressure rise rate.

[0021] Further preferably, the specific method of vacuuming and measuring the pressure rise rate is: vacuuming for 15 to 20 minutes, pumping the pressure to below 100Pa, closing the baffle valve, and turning off the vacuum pump; waiting for 1 hour to obtain the final pressure value; if the pressure rise rate result is ≤600Pa, production can continue; if it is greater than 600Pa, production is stopped and the equipment needs to be leak tested.

[0022] Preferably, MTS is heated to 50° C. to convert it from liquid to gas, and then mixed with argon and hydrogen.

[0023] Preferably, the pressure is controlled to be 2000-3000 Pa during the chemical vapor deposition process.

[0024] Preferably, after the deposition is completed, the mixed gas is stopped, the vacuum is evacuated to 100 Pa, the heating is stopped, the mixture is naturally cooled to 600°C, nitrogen is introduced to a slightly positive pressure, the mixture is further naturally cooled to room temperature, nitrogen is introduced for replacement, and the product is taken out.

[0025] The present invention also provides silicon carbide whiskers prepared by the above method.

[0026] The present invention also provides the use of the aforementioned silicon carbide whisker as a reinforcing and toughening agent for ceramic-based or metal-based composite materials.

[0027] The present invention has the following beneficial effects:

[0028] The present invention uses silicon carbide fiber as a matrix and obtains silicon carbide whiskers by chemical vapor deposition. The present invention controls the purity of the raw material methyltrichlorosilane MTS, as well as the mixed gas flow ratio and temperature of chemical vapor deposition. Compared with the general CVD method, the process is simpler, the process is easy to control, and the silicon carbide whiskers finally obtained have high purity. The silicon carbide whiskers obtained by the present invention can be used for the reinforcement and toughening of ceramic-based or metal-based composite materials, and have good application prospects.

[0029] The present invention adopts chemical vapor deposition, uses MTS as the reaction gas, and passes H 2 Ar is the carrier gas 2 To protect the gas, SiC whiskers are grown on silicon carbide fibers at a specific temperature and pressure. The reaction formula is as follows:

[0030] CH 3 Cl 3 Si(gas)+H 2 (carrier)→SiC (whiskers)+HCl (gas).

[0031] The key factors for preparing high-purity whiskers generally include: MTS purity, reaction temperature, gas flow ratio, etc. The specific analysis is as follows:

[0032] 1. Purity of MTS:

[0033] The purity of the raw materials directly affects the purity of the whiskers. The higher the purity, the less impurities volatilized during the reaction, and the less by-products produced by deposition. The purity of MTS on the market generally includes industrial grade, electronic grade (4N, 6N), etc. Considering the cost issue, the purity of MTS selected in the present invention is 4N.

[0034] 2. Reaction temperature:

[0035] Low temperature deposition belongs to the range of reaction control process, with many defects, less impurity diffusion, smaller pattern drift, and a smooth plane. High temperature deposition belongs to the range of diffusion control process, with few defects, increased impurity diffusion, larger pattern drift, and a rough and uneven surface morphology. The present invention has determined the optimal temperature control process through continuous trial and screening.

[0036] The heating rate prevents the equipment from running at high load, thus improving the stability of the equipment. The insulation section can make the temperature in the deposition chamber more uniform and eliminate temperature differences.

[0037] The deposition temperature determines the diffusion, decomposition and deposition rate of the reaction gas. As the temperature increases, the diffusion coefficient decreases, the permeability decreases, and excessive surface deposition is likely to occur, making it difficult to generate silicon carbide nanowires. Lowering the temperature will reduce the deposition rate and extend the growth cycle.

[0038] Therefore, after a long period of orthogonal experiments, this heating curve is desirable.

[0039] 3. Gas flow ratio:

[0040] The size of the flow ratio affects the generated sediments. If the flow ratio is too small, the sediments are free carbon and β-SiC, while if the flow ratio is too large, the sediments are free silicon and β-SiC. 2 In this method, it is not only a diluent gas and a carrier gas, but also acts as a catalyst to affect the reaction rate and the formation of whiskers during the reaction.

[0041] The present invention does not require the deposition of a carbon interface phase, but directly deposits whiskers, which has a short preparation cycle, low cost, high efficiency, and few gas paths. Silicon carbide fibers are directly selected as the matrix, and more complex special-shaped parts can be made later through weaving, impregnation, cracking and other process means, which are not limited to the singleness of the product. The silicon carbide whiskers obtained by the present invention can be applied to high-temperature components in the fields of ceramics and aerospace. The parts made by adding the silicon carbide whiskers have better high temperature resistance and wear resistance, and can be widely used as structural materials in aviation, aerospace, automobiles, machinery, petrochemical and other industrial fields.

[0042] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0044] Figure 1This is a scanning electron microscope image of the deposited whiskers in Example 1, wherein A is 20,000 times under an electron microscope, B is 100 times under an electron microscope, C is 50,000 times under an electron microscope, and D is 5,000 times under an electron microscope. DETAILED DESCRIPTION

[0045] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, but the present invention can be implemented in many different ways as defined and covered by the claims.

[0046] The present invention uses a CVD deposition furnace developed and produced by the Hunan Carbon Source Technology Co., Ltd. team to prepare silicon carbide whiskers. The silicon carbide fiber is Ze Rui 200 or Ze Rui 201, and the tow is 500 or 1000.

[0047] Embodiment 1:

[0048] A method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material, the specific steps are as follows:

[0049] (1) Furnace loading: clean the furnace, wind the silicon carbide fiber regularly on the tooling of the graphite material table (i.e. the loading table in the furnace) (the winding requirement is to be evenly distributed on the tooling, and the fibers cannot overlap), and close the furnace door.

[0050] (2) Vacuum and measure the pressure rise rate: Vacuum for 15-20 minutes until the pressure is below 100Pa, close the baffle valve, and turn off the vacuum pump. Wait for 1 hour to get the final pressure value. If the pressure rise rate result is ≤600Pa, production can continue. If it is greater than 600Pa, production should be stopped and the equipment should be leak tested.

[0051] (3) Heating:

[0052] Room temperature - 600℃ 1.5h

[0053] 600℃-600℃1h(heat preservation section)

[0054] 600℃-1100℃2h

[0055] 1100℃-1100℃2h(heat preservation stage)

[0056] 1100℃-1100℃4h(deposition stage)

[0057] (4) Start the MTS heating system to convert the liquid into gas.

[0058] (5) Gas introduction: Argon 3 L / min, hydrogen 6 L / min and MTS 1 L / min were introduced into the gas mixing tank in sequence according to the flow ratio until the pressure was slightly positive and then steadily introduced into the deposition chamber. The pressure in the deposition chamber was 1500-3000 Pa.

[0059] (6) After the deposition is completed and the deposition time is reached stably, ventilation is stopped, vacuum is evacuated to below 100 Pa, heating is stopped, and automatic cooling is performed.

[0060] (7) Cooling: The temperature is lowered to below 600°C and nitrogen is introduced to a slightly positive pressure.

[0061] (8) Taking out of the furnace: After the temperature drops to room temperature and nitrogen is introduced for replacement, the furnace bottom is opened as required to take out the workpiece.

[0062] Scanning electron microscopy images of deposited whiskers are shown in Figure 1 , the values ​​on the figure are the whisker diameters randomly selected within the field of view.

[0063] Embodiment 2:

[0064] A method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material, the specific steps are as follows:

[0065] (1) Furnace loading: clean the furnace, wind the silicon carbide fiber regularly on the tooling of the graphite material table, and close the furnace door.

[0066] (2) Vacuum and measure the pressure rise rate: Vacuum for 15-20 minutes until the pressure is below 100Pa, close the baffle valve, and turn off the vacuum pump. Wait for 1 hour to get the final pressure value. If the pressure rise rate result is ≤600Pa, production can continue. If it is greater than 600Pa, production should be stopped and the equipment should be leak tested.

[0067] (3) Heating:

[0068] Room temperature - 600℃ 1.5h

[0069] 600℃-600℃1h(heat preservation section)

[0070] 600℃-1200℃3h

[0071] 1200℃-1200℃2h(heat preservation stage)

[0072] 1200℃-1200℃2h(deposition stage)

[0073] (4) Start the MTS heating system to convert the liquid into gas.

[0074] (5) Introducing gas: According to the flow ratio, introduce argon 6L / min, hydrogen 12L / min and MTS 2L / min into the mixing tank in sequence until the pressure is slightly positive, and then steadily introduce it into the deposition chamber. The pressure in the deposition chamber is 1500-3000Pa.

[0075] (6) After the deposition is completed and the deposition time is reached stably, ventilation is stopped, vacuum is evacuated to below 100 Pa, heating is stopped, and automatic cooling is performed.

[0076] (7) Cooling: The temperature is lowered to below 600°C and nitrogen is introduced to a slightly positive pressure.

[0077] (8) Taking out of the furnace: After the temperature drops to room temperature and nitrogen is introduced for replacement, the furnace bottom is opened as required to take out the workpiece.

[0078] Embodiment 3:

[0079] A method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material, the specific steps are as follows:

[0080] (1) Furnace loading: clean the furnace, wind the silicon carbide fiber regularly on the tooling of the graphite material table, and close the furnace door.

[0081] (2) Vacuum and measure the pressure rise rate: Vacuum for 15-20 minutes until the pressure is below 100Pa, close the baffle valve, and turn off the vacuum pump. Wait for 1 hour to get the final pressure value. If the pressure rise rate result is ≤600Pa, production can continue. If it is greater than 600Pa, production should be stopped and the equipment should be leak tested.

[0082] (3) Heating:

[0083] Room temperature - 600℃ 1.5h

[0084] 600℃-600℃1h(heat preservation section)

[0085] 600℃-950℃2h

[0086] 950℃-950℃2h(heat preservation period)

[0087] 950℃-950℃4h(deposition stage)

[0088] (4) Start the MTS heating system to convert the liquid into gas.

[0089] (5) Gas introduction: Argon (4.5 L / min), hydrogen (9 L / min) and MTS (1.5 L / min) were introduced into the gas mixing tank in sequence according to the flow ratio until the pressure reached a slightly positive pressure and then steadily introduced into the deposition chamber.

[0090] (6) After the deposition is completed and the deposition time is reached stably, ventilation is stopped, vacuum is evacuated to below 100 Pa, heating is stopped, and automatic cooling is performed.

[0091] (7) Cooling: The temperature is lowered to below 600°C and nitrogen is introduced to a slightly positive pressure.

[0092] (8) Taking out of the furnace: After the temperature drops to room temperature and nitrogen is introduced for replacement, the furnace bottom is opened as required to take out the workpiece.

[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing silicon carbide whiskers by chemical vapor deposition using MTS as a raw material, characterized in that: Silicon carbide fibers were used as the matrix and chemical vapor deposition was performed to obtain silicon carbide whiskers. A mixed gas of argon, hydrogen and methyltrichlorosilane (MTS) was introduced into the chemical vapor deposition, and the flow rates of the three gases were 3-6 L / min, 6-12 L / min and 1-2 L / min, respectively. The temperature of the chemical vapor deposition was controlled as follows: (A) uniformly heating from room temperature to 600°C over 1.5 to 2 hours and keeping the temperature for 1 to 2 hours; (B) Continue to raise the temperature to 950-1200° C. over 2-3 hours and keep it at that temperature for 2 hours; (C) deposition at 950-1200°C for 2-4 hours; The pressure is controlled at 2000-3000Pa during the chemical vapor deposition process.

2. The method according to claim 1, characterized in that The flow rates of argon, hydrogen and methyltrichlorosilane MTS were 3 L / min, 6 L / min and 1 L / min respectively.

3. The method according to claim 1, characterized in that The purity of the MTS is 4N.

4. The method according to claim 1, characterized in that: The temperature of chemical vapor deposition is controlled as follows: (A) The temperature is raised uniformly from room temperature to 600°C over 1.5 hours and kept at this temperature for 1 hour; (B) Continue to raise the temperature to 1100°C over 2 hours and keep it at that temperature for 2 hours; (C) Deposition at 1100°C for 4 hours.

5. The method according to claim 1, characterized in that: Use a CVD deposition furnace to carry out chemical vapor deposition, clean the furnace chamber, wind the silicon carbide fiber regularly on the tooling of the graphite material table, close the furnace door, evacuate the furnace, and measure the pressure rise rate.

6. The method according to claim 1, characterized in that MTS is heated to 50°C to convert it from liquid to gas, and then mixed with argon and hydrogen.

7. The method according to claim 1, characterized in that After the deposition is completed, stop introducing the mixed gas, evacuate to 100Pa, stop heating, cool naturally to 600℃, introduce nitrogen to a slightly positive pressure, continue to cool naturally to room temperature, introduce nitrogen for replacement, and take out the product.