A preparation method and production system of high-strength aluminum alloy profile
By using a heat treatment process of low-temperature extrusion combined with rapid heating in 6XXX series aluminum alloy, the heat treatment temperature and temperature increase rate are controlled, and the strength and thickness of the coarse crystal layer caused by the recrystallization and quenching transfer time of the material during the extrusion process is solved, and the thickness of the coarse crystal layer is achieved. The high yield strength and resistance to intergranular corrosion are improved, and the yield rate is improved.
Patent Information
- Application Number
- CN202410627036.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-21
AI Technical Summary
The existing 6XXX series aluminum alloys are difficult to have high yield strength and thin coarse crystal layer thickness during the extrusion process due to their high quenching sensitivity. In conventional processes, the material results in strength loss during the quenching transfer time.
The heat treatment process of low-temperature extrusion combined with rapid heating is adopted. The extruded profile is heated through the heat treatment device to control the heat treatment temperature and heating rate, ensuring that the material recrystallizes in a small amount or does not crystallize during the extrusion process, and reduces the coarse crystal layer. Thickness and enhance material strength and intergranular corrosion resistance through water spray cooling and tensile straightening.
Improve the yield strength and corrosion resistance of the material, reduce the strength loss caused by quenching transfer time, ensure the consistent temperature of the profile head, middle and tail, and improve the material yield, especially the large-section size profile, which significantly improves the material yield. .
Smart Images

Figure CN118204385B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy manufacturing, and specifically relates to a preparation method of a high-strength aluminum alloy profile and a production system thereof. Background Art
[0002] With the continuous development of industry, higher requirements are put forward for the performance of industrial aluminum profiles (such as product strength performance, corrosion resistance, service performance, etc.). 6XXX series aluminum alloy is currently commonly used industrial aluminum alloy profiles. It is a heat-treatable alloy that can improve material strength by precipitating strengthening phases through heat treatment.
[0003] In order to improve the mechanical properties of this type of aluminum alloy, the extrusion rod temperature and extrusion speed are usually increased during the extrusion process to achieve the purpose of the outlet temperature reaching the solution temperature. Since the high temperature period during the extrusion process is short, and the quenching sensitivity of the 6XXX series aluminum alloy is high, the quenching transfer time requirement is short, and the 6XXX aluminum alloy does not have sufficient solution time during the conventional extrusion process, the extrusion outlet temperature can only be further increased to even the overburning temperature to achieve online quenching of the 6XXX series aluminum alloy. Although some researchers have used a heat preservation device to keep the extruded material warm on this basis to increase the solution time and avoid the temperature drop of the material before entering the quenching section, the use of a heat preservation device is likely to increase the surface coarse grain layer thickness and intergranular corrosion depth that affect the service performance of the material.
[0004] Although the addition of transition elements such as Mn and Cr to form a dispersed phase can achieve a certain effect of inhibiting recrystallization, when the temperature is high, the dispersed phase containing Mn and Cr elements will become coarse and cannot effectively pin dislocations. The grains tend to coarsen and the surface coarse-grained layer cannot be effectively improved. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a high-strength aluminum alloy profile and a production system thereof which can simultaneously improve material strength, surface quality and yield rate.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a high-strength aluminum alloy profile comprises feeding an aluminum alloy substrate into an extruder for extrusion molding to obtain a profile, and then sequentially performing online quenching, stretching straightening and artificial aging on the profile, the preparation method further comprising allowing the profile to enter a heat treatment device for heating treatment after exiting the extruder, and then performing the online quenching, stretching straightening and artificial aging on the profile after the heating treatment,
[0008] The aluminum alloy substrate is selected from any one of 6XXX series aluminum alloys,
[0009] The temperature of the profile at the discharge port of the heat treatment device is controlled to be greater than the temperature of the profile at the discharge port of the extruder and the difference between the two is more than 10°C. The temperature of the profile at the discharge port of the heat treatment device is not less than 530°C. The average heating rate of the profile during the heating treatment is controlled to be 0.5~4.5°C / s.
[0010] Too low an extrusion temperature will not only make forming more difficult, but also prevent the strengthening phases (β'', β' phases) in the alloy from being fully dissolved, thus affecting the final material strength, especially the yield strength. Even if the material strength can be improved to a certain extent through subsequent quenching and artificial aging processes, the improvement is limited. Therefore, in order to obtain higher-strength 6XXX series aluminum alloys, the prior art often increases the extrusion temperature to the complete solution temperature to promote the full solution of the strengthening phase. Some researchers will also use a heat preservation device to increase the solution time on this basis. Although these methods can improve the strength of the material, they will lead to an increase in the degree of dynamic recrystallization on the surface of the material and an increase in the thickness of the coarse-grained layer. Therefore, it is difficult for the existing 6XXX series aluminum alloys to have both high yield strength and thin coarse-grained layer thickness. Unexpectedly, when the extrusion temperature is lower and the heat treatment temperature is higher, the material strength and the thickness of the coarse-grained layer can be improved. The inventor speculates that the relatively low extrusion temperature reduces the dynamic recrystallization of the material surface during extrusion, and at the same time, the Mg in the material 2 Si metastable phase is generated, and some Mg 2 The Si metastable phase has the effect of hindering the movement of grain boundaries. Therefore, when the material passes through the extruder to the heat treatment device, the internal structure can recover and the recrystallization energy storage consumes more. Even if the heat treatment device reaches a higher temperature, the structure does not grow by recrystallization, which can not only ensure the strength of the material, but also reduce the thickness of the coarse grain layer.
[0011] As the difference between the heat treatment temperature and the extrusion temperature increases, the material performance is further improved, but as the difference between the two increases further, the thickness of the coarse-grained layer of the material increases. Therefore, as a preference, the difference between the profile temperature at the discharge port of the heat treatment device and the profile temperature at the discharge port of the extruder does not exceed 40°C. In addition, a faster heating rate or a slower heating rate will lead to a thicker coarse-grained layer. The present invention further reduces the thickness of the coarse-grained layer by controlling the heating rate.
[0012] Preferably, the average heating rate of the profile during the heating treatment is controlled to be 1.5~3.0℃ / s, for example, 1.5℃ / s, 1.8℃ / s, 2.0℃ / s, 2.3℃ / s, 2.5℃ / s, 2.8℃ / s or 3.0℃ / s.
[0013] Preferably, the heating treatment time is 10-20 seconds, such as 10 seconds, 12 seconds, 14 seconds, 16 seconds, 18 seconds or 20 seconds. A faster heating rate (1.5-3.0°C / s) combined with a shorter heating time (10-20 seconds) can further reduce the thickness of the coarse-grained layer of the 6XXX series aluminum alloy and improve the material's resistance to intergranular corrosion.
[0014] Preferably, the profile temperature at the discharge port of the heat treatment device is 540-570°C, more preferably 545-560°C, for example 545°C, 550°C, 555°C or 560°C.
[0015] Preferably, in the extrusion molding process, the temperature of the aluminum alloy substrate is controlled to be 475-495° C., the die heating temperature of the extruder is controlled to be 460-480° C., the extrusion speed is controlled to be 1-5 mm / s, and the extrusion ratio is controlled to be 15-45.
[0016] Further preferably, in the extrusion molding process, the temperature of the aluminum alloy substrate is controlled to be 480-490° C., the die heating temperature of the extruder is controlled to be 465-475° C., the extrusion speed is controlled to be 2-4 mm / s, and the extrusion ratio is controlled to be 25-35.
[0017] Preferably, the 6XXX series aluminum alloy includes 6005 aluminum alloy, 6061 aluminum alloy and 6082 aluminum alloy.
[0018] In some implementations, when the aluminum alloy substrate is 6005 aluminum alloy, the profile temperature at the discharge port of the extruder is controlled to be 515-525°C, and the profile temperature at the discharge port of the heat treatment device is controlled to be 540-560°C.
[0019] In some implementations, when the aluminum alloy substrate is 6061 aluminum alloy, the profile temperature at the discharge port of the extruder is controlled to be 525-535° C., and the profile temperature at the discharge port of the heat treatment device is controlled to be 545-570° C.
[0020] In some implementations, when the aluminum alloy substrate is 6082 aluminum alloy, the profile temperature at the discharge port of the extruder is controlled to be 530-540°C, and the profile temperature at the discharge port of the heat treatment device is controlled to be 545-570°C.
[0021] Preferably, the online quenching includes cooling the heat-treated profile to below 100° C. within 0.2 to 0.5 min using water spray cooling.
[0022] Preferably, the stretching amount of the stretching straightening is controlled within 0.2%.
[0023] Preferably, the artificial aging system is 185±10°C, 4~8h.
[0024] The present invention also provides a production system for high-strength aluminum alloy profiles, the production system comprising a control module, an extruder for extruding an aluminum alloy substrate, a heat treatment device for heating the profile and controlled by the control module, and a quenching module for spraying water to cool the profile, the heat treatment device being between the extruder and the quenching module, and comprising a support mechanism and a heating furnace and a guide mechanism arranged on the support mechanism.
[0025] The heating furnace comprises a furnace body, a heating nozzle and a heating assembly, wherein the furnace body has a heating cavity for passing a profile and extending along the length direction of the furnace body, a cavity is formed between the inner wall of the heating cavity and the outer shell of the furnace body, the heating nozzle has a plurality of nozzles distributed on the inner wall of the heating cavity, the heating nozzle is connected to the cavity and the length and angle of the nozzle extending out of the inner wall of the heating cavity are adjustable, the heating assembly is connected to the furnace body, and comprises a heating element for heating and a circulating fan for sending the heat generated by the heating element into the heating cavity through the heating nozzle;
[0026] The guide mechanism is used to align the profile entering the heating cavity in the up-down and left-right directions. The guide mechanism has two groups arranged on the front and rear sides of the heating furnace. Each group of guide mechanisms includes a guide rail connected to the support mechanism and extending along the width direction of the furnace body, a first guide roller and a second guide roller slidingly arranged on the guide rail, a driving member connected to the first guide roller and the second guide roller and used to drive the first guide roller and the second guide roller to move closer to or away from each other so as to align the profile located between the first guide roller and the second guide roller in the left-right direction, and a support roller connected to the support mechanism and parallel to the guide rail and used to align the profile located thereon in the up-down direction.
[0027] Preferably, the heating nozzle is in the shape of a bellows.
[0028] Preferably, the heating nozzles have multiple rows evenly distributed along the circumference of the heating cavity, each row of heating nozzles has multiple heating nozzles evenly arranged along the length direction of the heating cavity, and the heating nozzles in two adjacent rows are staggered.
[0029] Preferably, the cross section of the heating channel perpendicular to its length direction is circular.
[0030] Preferably, the furnace body comprises a lower furnace body and an upper furnace body covering the lower furnace body and hinged to the lower furnace body, and the middle areas of the upper furnace body and the lower furnace body are recessed inwards and the heating cavity is formed therebetween.
[0031] Preferably, the length of the furnace body is 0.5-2 m.
[0032] Preferably, the heating furnace further comprises a temperature monitoring device disposed on the furnace body and used for monitoring the temperature of the furnace body.
[0033] Preferably, the heating element is heated by electricity or natural gas.
[0034] Preferably, the production system further comprises a first temperature detector for monitoring the temperature at the discharge port of the extruder and a second temperature detector for detecting the temperature at the discharge port of the heating furnace.
[0035] Preferably, the production system further comprises an air knife arranged between the heat treatment device and the quenching module, wherein the air knife faces the feed port of the quenching module to ensure that water mist in the quenching zone does not enter the furnace body.
[0036] The production system of the present invention has a simple structure, a fast heating rate of the heat treatment device, and uniform temperature control, which can achieve uniform temperature of the material cross section, improve the uneven temperature of each surface of the material in the extrusion die due to different extrusion conditions, and the phenomenon of quenching deformation caused by different cooling rates during the quenching process. In particular, the phenomenon of large water quenching deformation of materials with high quenching sensitivity can be greatly improved.
[0037] The present invention also provides a method for producing high-strength aluminum alloy using the production system as described above, comprising feeding an aluminum alloy substrate into an extruder for extrusion molding to obtain a profile, and then allowing the profile to enter a heat treatment device for heating treatment after exiting the extruder, and then allowing the profile to enter a quenching module for water spray cooling after exiting the heat treatment device.
[0038] Preferably, when the heat treatment is performed, the heating nozzle of the heat treatment device is directed toward the profile and the distance between it and the profile is 70 to 90 mm. The control module adjusts the gas flow rate and wind pressure of the heating nozzle according to the profile temperature at the discharge port of the extruder and the heat treatment device so that the profile temperature at the discharge port of the extruder and the heat treatment device is consistent with the set value.
[0039] Preferably, the gas flow rate of the heating nozzle is 500-700 m 3 / min, wind pressure is 800~1000kPa.
[0040] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0041] The present invention adds a heat treatment device at the extrusion outlet. For 6XXX series aluminum alloys, a relatively low extrusion outlet temperature is combined with a heat treatment device to quickly heat the extruded profile, ensuring that a small amount of recrystallization or no recrystallization occurs in the profile during the extrusion process, reducing the thickness of the coarse-grained layer on the surface of the profile, and improving the material's resistance to intergranular corrosion. The subsequent rapid heating process increases the thickness of the coarse-grained layer by a small amount, but can quickly dissolve the matrix Mg 2 Si can increase the strength of the material and further improve the material's resistance to intergranular corrosion.
[0042] The preparation method of the present invention reduces or even substantially eliminates the quenching transfer time, thereby avoiding the strength loss of the material caused by the quenching transfer time.
[0043] In addition, during the extrusion and rod changing process, the tail material is heated and insulated by the heat treatment device and is always at the solid solution temperature. The material properties do not decrease, which can ensure that the temperature of the head, middle and tail of the profile is consistent and the performance fluctuation is smaller. It can also ensure that the mechanical properties of the head and tail of the profile are qualified, thereby improving the material yield rate, especially for profiles with large cross-section sizes, the material yield rate can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a structural schematic diagram of a production system of a high-strength aluminum alloy profile of the present invention;
[0045] Figure 2 It is a structural schematic diagram of a heat treatment device of the present invention;
[0046] Figure 3 A top view of a lower furnace body of the present invention;
[0047] Figure 4 It is a structural schematic diagram of a heating nozzle of the present invention;
[0048] Figure 5 Schematic diagram of the thickness of the coarse-grained layer of the profile obtained in Example 1;
[0049] Figure 6 Schematic diagram of the thickness of the coarse-grained layer of the profile obtained in Comparative Example 2;
[0050] Figure 7 Schematic diagram of intergranular corrosion depth of the profile obtained in Example 1;
[0051] Figure 8 Schematic diagram of intergranular corrosion depth of the profile obtained in Comparative Example 2;
[0052] Fig. 9 This is a physical picture of the profile obtained in Example 1. The product surface is smooth and has no twisting or deformation;
[0053] Fig.10This is a physical picture of the profile obtained in Comparative Example 2, with aluminum nodules and mold marks appearing on the surface of the product;
[0054] Fig.11 This is another physical picture of the profile obtained in Comparative Example 2. The product is twisted and deformed after quenching;
[0055] Among them, 1. Extruder;
[0056] 2. Heat treatment device; 21. Support mechanism; 22. Lower furnace body; 23. Upper furnace body; 24. Heating cavity; 241. Inner wall of heating cavity; 25. Heating nozzle; 26. Guide mechanism; 261. Guide rail; 262. First guide roller; 263. Second guide roller; 264. Support roller; 2641. Support member; 2642. Roller body;
[0057] 3. Quenching module;
[0058] 41. a first temperature detector; 42. a second temperature detector;
[0059] 5. Profile. DETAILED DESCRIPTION
[0060] In order to improve the mechanical properties of aluminum alloys, a high-temperature extrusion process is usually used, that is, to increase the temperature of the profile at the discharge port of the extruder. This method will cause the surface quality of the material to decrease, and the temperature of the profile will inevitably decrease before entering the quenching section, which will cause the mechanical properties of the material to decrease. Although some researchers have used an insulation device to keep the temperature after extrusion in order to avoid temperature reduction, the performance of the obtained aluminum alloy still needs to be improved. The inventors used a low-temperature extrusion process combined with a rapid heating heat treatment process for 6XXX series aluminum alloys to reduce the formation of a coarse-grained layer on the surface of the material while allowing a large amount of precipitated phases inside the material to dissolve back, thereby improving the material properties. The profiles obtained by the method of the present invention have high strength, good surface quality, high yield rate, small deformation, no defects such as sticky aluminum, aluminum nodules, microcracks, and good appearance. In addition, the inventors have also designed a production system for high-strength aluminum alloy profiles, as follows.
[0061] like Figure 1 As shown, the production system of the high-strength aluminum alloy profile of the present invention comprises a control module, an extruder 1 for extruding an aluminum alloy substrate, a heat treatment device 2 for heating the profile 5 and controlled by the control module, and a quenching module 3 for spraying water to cool the profile 5, wherein the heat treatment device 2 is located between the extruder 1 and the quenching module 3 and is arranged adjacent to the extruder 1 and the quenching module 3. Among them, the control module, the extruder 1 and the quenching module 3 refer to the prior art, and the present invention does not focus on them, and the heat treatment device 2 is described in detail below.
[0062] like Figure 2As shown, the heat treatment device 2 includes a support mechanism 21 , a heating furnace and a guide mechanism 26 arranged on the support mechanism 21 .
[0063] The heating furnace comprises a furnace body, a heating nozzle 25 and a heating assembly.
[0064] The furnace body has a heating cavity 24 for passing the profile 5 and extending along the length direction of the furnace body. A chamber (not shown in the figure) is formed between the inner wall 241 of the heating cavity and the outer shell of the furnace body. The cross section of the heating cavity 24 perpendicular to its length direction is circular. Specifically, the furnace body includes a lower furnace body 22 and an upper furnace body 23 covering the lower furnace body 22 and hinged to the lower furnace body 22. The middle area of the upper furnace body 23 and the lower furnace body 22 is concave inward and the heating cavity 24 is formed between the two. The length of the furnace body is 0.5~2m. In the following text, if there is no special explanation, the furnace body length used is 1.2m.
[0065] like Figure 3 As shown, the heating nozzles 25 have multiple rows evenly distributed along the circumference of the heating channel 24, each row of heating nozzles 25 has multiple heating nozzles 25 evenly arranged along the length direction of the heating channel 24, and the heating nozzles 25 in two adjacent rows are staggered. Take one of the heating nozzles 25 as an example, Figure 4 As shown, the heating nozzle 25 is in the shape of a bellows. The design of the bellows-shaped heating nozzle 25 facilitates adjustment of the length and angle of the heating nozzle 25 extending out of the inner wall 241 of the heating cavity, so that the nozzle direction and length can be adjusted according to the different sections of the profile 5 for different wall thicknesses, so that the thick wall area is concentratedly heated to ensure uniform temperature of the entire cross section. Usually, it is best to make the heating nozzle 25 face the surface of the profile 5 and the distance between the heating nozzle 25 and the profile 5 is 80±10mm. One end of the heating nozzle 25 is connected to the inner wall 241 of the heating cavity by screws and spot welding and is connected to the corresponding furnace body, and the other end is open for air discharge to heat or keep the profile 5 warm.
[0066] The heating assembly (not shown) is connected to the furnace body, and includes a heating element for heating and a circulating fan for delivering the heat generated by the heating element into the heating cavity 24 through the heating nozzle 25. The heating element includes but is not limited to electric heating and natural gas heating, and the details can be referred to the prior art.
[0067] The guide mechanism 26 is used to center the profile 5 entering the heating cavity 24 in the vertical direction and the left-right direction. It has two groups located at the front and rear sides of the heating furnace. Each group of the guide mechanism 26 includes a guide rail 261 connected to the support mechanism 21 and extending in the width direction of the furnace body, a first guide roller 262 and a second guide roller 263 slidably arranged on the guide rail 261, a driving member (not shown in the figure, the driving member can be a motor, for example) connected to the first guide roller 262 and the second guide roller 263 and used to drive the first guide roller 262 and the second guide roller 263 to move closer to or away from each other so as to center the profile 5 located between the first guide roller 262 and the second guide roller 263 in the left-right direction, and a support roller 264 connected to the support mechanism 21 and parallel to the guide rail 261 and used to center the profile 5 located thereon in the vertical direction. The support roller 264 includes a support member 2641 connected to the support mechanism 21 and a roller body 2642 rotatably arranged in the middle area of the support member 2641. The bearing surface of the roller body 2642 is substantially at the same height as the axis of the heating chamber 24, so as to vertically center the profile 5 on the roller body 2642. The support roller 264 is located between the corresponding guide rail 261 and the furnace body.
[0068] The heating furnace also includes a temperature monitoring device arranged on the furnace body and used to monitor the temperature of the furnace body, and the temperature detection device is connected to the control system. Preferably, the temperature monitoring device is a thermocouple.
[0069] The support mechanism 21 includes a first portion for supporting the front guide assembly, a second portion for supporting the heating furnace, and a third portion for supporting the rear guide assembly. Usually, the first portion and the third portion are of the same height and both are higher than the second portion to ensure that the profile 5 runs in the center of the heating furnace. The support mechanism 21 can be constructed of a steel frame.
[0070] The production system further comprises a first temperature detector 41 for monitoring the temperature at the discharge port of the extruder 1 and a second temperature detector 42 for detecting the temperature at the discharge port of the heating furnace.
[0071] The present invention is further described below in conjunction with the examples. However, the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.
[0072] Unless otherwise specified, the raw materials mentioned in this article are all commercially available products in the field. Example 1
[0073] A method for preparing a high-strength aluminum alloy profile comprises using the above production system to prepare the high-strength aluminum alloy profile, and specifically comprises the following steps:
[0074] (1) A 6005 aluminum rod is fed into an extrusion die of an extruder 1 for extrusion molding to obtain a profile, wherein the aluminum rod temperature is 480-490°C, the extrusion die heating temperature is 470°C, the extrusion speed is 3 mm / s, the extrusion ratio is 30, and the profile outlet temperature is 520°C;
[0075] (2) The extruded profile is directly centered by the guide mechanism 26 at the feed port of the heat treatment device 2 and then enters the heating furnace. It moves from the feed port of the heating furnace toward the discharge port at a certain speed (usually the profile speed = extrusion speed × extrusion ratio, that is, the profile speed in this embodiment is 90 mm / s). The gas flow rate and wind pressure of the heating nozzle 25 are adjusted according to the first temperature detector 41, the second temperature detector 42 and the temperature monitoring device so that the profile outlet temperature is 550°C and the average profile heating rate is 2.25°C / s (usually the average profile heating rate = (profile temperature at the discharge port of the heat treatment device 2 - profile temperature at the discharge port of the extruder 1) × profile speed / heating furnace length). In this embodiment, the gas flow rate of the heating nozzle 25 is 600±20m 3 / min, wind pressure is 900±5 kPa;
[0076] (3) The profile enters the quenching unit through the guide mechanism 26 at the outlet of the heat treatment device 2 for water spray cooling, so that the profile is cooled to a temperature of ≤100°C within 0.5 min;
[0077] (4) Send the cooled profile to the traction straightening machine for stretching and straightening, and the stretching amount is controlled within 0.2%;
[0078] (5) The profile after stretching and straightening was artificially aged at 185°C for 6 h to obtain an aluminum alloy profile with a thickness of 2.5 mm and a length of 28 m. Example 2
[0079] This embodiment is substantially the same as Embodiment 1, except that:
[0080] In step (2), the gas flow rate and wind pressure of the heating nozzle 25 are adjusted so that the profile outlet temperature is 530°C and the average profile heating rate is 0.75°C / s. Example 3
[0081] This embodiment is substantially the same as Embodiment 1, except that:
[0082] In step (2), the gas flow rate and wind pressure of the heating nozzle 25 are adjusted so that the profile outlet temperature is 560°C and the average profile heating rate is 3.0°C / s. Example 4
[0083] This embodiment is substantially the same as Embodiment 1, except that:
[0084] In step (2), the gas flow rate and wind pressure of the heating nozzle 25 are adjusted so that the profile outlet temperature is 540°C and the average profile heating rate is 1.5°C / s. Example 5
[0085] This embodiment is substantially the same as Embodiment 1, except that:
[0086] Step (2) adjusts the gas flow rate and wind pressure of the heating nozzle 25 and the length of the furnace body so that the profile outlet temperature is 550°C and the average profile heating rate is 0.5°C / s.
[0087] Comparative Example 1
[0088] This comparative example is substantially the same as Example 1, except that:
[0089] After step (1), step (3) is directly performed without going through step (2).
[0090] Comparative Example 2
[0091] This comparative example is substantially the same as Example 1, except that:
[0092] In step (1), the temperature of the aluminum rod is 500-510°C, the heating temperature of the extrusion die is 480-490°C, and the profile outlet temperature is 550°C;
[0093] After step (1), step (2) is skipped and step (3) is directly performed.
[0094] Comparative Example 3
[0095] This comparative example is substantially the same as Example 1, except that step (1) and step (2) are different, as follows:
[0096] Step (1): feeding a 6005 aluminum rod into an extrusion die of an extruder 1 for extrusion molding to obtain a profile, wherein the aluminum rod temperature is 500-510°C, the extrusion die heating temperature is 480-490°C, the extrusion speed is 3 mm / s, the extrusion ratio is 30, and the profile outlet temperature is 550°C;
[0097] Step (2): The extruded profile is directly centered by the guide mechanism 26 at the feed inlet of the heat treatment device 2 and then enters the heating furnace. It moves from the feed inlet of the heating furnace to the discharge port at a certain speed. The gas flow rate and wind pressure of the heating nozzle 25 are adjusted according to the feed inlet temperature detector and the discharge port temperature detector to keep the profile at 550°C.
[0098] The performance tests were conducted on the profiles prepared in the above embodiments and comparative examples. The test results are shown in Table 1.
[0099]
[0100] The test method for yield strength is based on ISO 6892-1 Metallic Materials-Tensile Test; the coarse grain layer thickness is determined by referring to the existing technology in the field, specifically, it can be measured by a microscope, 3 to 4 positions are selected in the coarse grain layer area to measure the thickness, and the average value is calculated as the coarse grain layer thickness; the test method for intergranular corrosion depth is based on GB / T 7998-2005 Determination method for intergranular corrosion of aluminum alloys.
[0101] For 6005 aluminum alloy, the low extrusion outlet temperature is not conducive to the improvement of the yield strength of the profile (such as comparative example 1). Although increasing the extrusion outlet temperature can improve the yield strength of the profile, it will increase the thickness of the coarse grain layer and the depth of intergranular corrosion of the profile, affecting the service performance and intergranular corrosion resistance of the profile (such as comparative example 2). At present, in order to improve the yield strength of the profile, the process of comparative example 2 is generally adopted. Further on the basis of comparative example 2, the profile is heat treated after extrusion, which is helpful to improve the yield strength of the profile, but it will significantly increase the thickness of the coarse grain layer and the depth of intergranular corrosion of the profile (such as comparative example 3). Unexpectedly, referring to Examples 1 to 5, by using a relatively low extrusion outlet temperature combined with a heat treatment device 2 to quickly heat the profile to the solution temperature after the extrusion, the yield strength of the profile can be improved while reducing the thickness of the coarse grain layer and the depth of intergranular corrosion. For 6005 aluminum alloy, the profile performance is optimal when the extrusion outlet temperature is 520℃, the heat-treated material outlet temperature is 550℃, and the average heating rate of the heat-treated profile is 2.25℃ / s.
[0102] The inventors speculate that by using low-temperature extrusion, the degree of dynamic recrystallization on the material surface is low, a small amount of recrystallization or no recrystallization occurs in the material during the extrusion process, and there are dispersed phases and Mg in the material that inhibit recrystallization from occurring after passing through the extruder to the heating furnace feed port. 2 Si metastable phase, recovery occurred inside the organization, and the recrystallization energy storage consumed a lot. Although it reached a higher temperature after the heating device, the organization did not recrystallize and grow, so the thickness of the coarse grain layer was thin. However, the traditional process (Comparative Example 2) has a high extrusion outlet temperature, and a large amount of dynamic recrystallization occurs in the material at the working zone. From the outlet of the extruder 1 to the quenching unit, a large amount of recrystallization and growth occurs in the material under high temperature, resulting in a thicker coarse grain layer under this process. The thickness of the coarse grain layer and the difference in internal organization lead to a significant change in the material's resistance to intergranular corrosion. The material in the embodiment has a thin coarse grain layer, and the material shows a recovery organization inside, and the resistance to intergranular corrosion is significantly better than the traditional process performance.
[0103] The inventors also compared the material properties of the head, middle and tail of the profiles of Example 1 and Comparative Example 2 along the length direction, and calculated the yield rate, see Table 2 and Table 3 for details.
[0104]
[0105]
[0106] It can be seen from Table 2 and Table 3 that the profile of Example 1 has higher strength and better consistency, and a higher yield rate.
[0107] In addition to the 6005 alloy, the inventors also conducted corresponding research on the 6061 alloy and the 6082 alloy, as follows. Example 6
[0108] This embodiment is substantially the same as embodiment 1, except that: step (1) uses a 6061 aluminum rod and the profile outlet temperature is 530°C.
[0109] Comparative Example 4
[0110] This comparative example is substantially the same as comparative example 1, except that: in step (1), a 6061 aluminum rod is used and the profile outlet temperature is 530°C.
[0111] Comparative Example 5
[0112] This comparative example is substantially the same as comparative example 2, except that a 6061 aluminum rod is used in step (1). Example 7
[0113] This embodiment is substantially the same as embodiment 1, except that: step (1) uses 6082 aluminum rods, and the profile outlet temperature is 535°C.
[0114] Comparative Example 6
[0115] This comparative example is substantially the same as comparative example 1, except that: in step (1), a 6082 aluminum rod is used and the profile outlet temperature is 535°C.
[0116] Comparative Example 7
[0117] This comparative example is substantially the same as comparative example 2, except that a 6082 aluminum rod is used in step (1).
[0118] The above-mentioned test method was used to perform performance tests on the profiles prepared in Examples 6 and 7 and Comparative Examples 4 to 7. The test results are shown in Table 4.
[0119]
[0120] As can be seen from Table 4, for 6061 aluminum alloy and 6082 aluminum alloy, using a relatively low extrusion outlet temperature in combination with heat treatment device 2 to quickly heat the profile to the solution temperature after extrusion can also improve the profile's yield strength, coarse grain layer thickness and intergranular corrosion resistance.
[0121] The inventors also compared the material properties of the head, middle and tail of the profiles of Example 6 and Comparative Example 5, and Example 7 and Comparative Example 7 along the length direction, and calculated the yield rate, see Table 5 and Table 6 for details.
[0122]
[0123] It can be seen from Table 5 and Table 6 that for 6061 aluminum alloy and 6082 aluminum alloy, the profiles prepared by the process of the present invention have higher strength and better consistency, and a higher yield rate.
[0124] In summary, the production process and production system of the present invention are not only conducive to obtaining higher strength 6XXX series aluminum alloy products, but also can improve product surface quality, increase material yield rate, and reduce production costs.
[0125] In addition to the research on 6XXX series aluminum alloys, the inventors also used the production system of the present application to prepare 7XXX series aluminum alloy profiles, as follows. Example 8
[0126] A method for preparing a high-strength aluminum alloy profile comprises using the above production system to prepare the high-strength aluminum alloy profile, and specifically comprises the following steps:
[0127] (1) Feeding a 7075 aluminum rod into an extrusion die of an extruder 1 for extrusion molding to obtain a profile, wherein the aluminum rod temperature is 420-430°C, the extrusion die heating temperature is 410-420°C, the extrusion speed is 2 mm / s, the extrusion ratio is 21, and the profile outlet temperature is 475°C;
[0128] (2) The extruded profile is directly centered by the guide mechanism 26 at the feed inlet of the heat treatment device 2 and then enters the heating furnace. It moves from the feed inlet of the heating furnace to the discharge outlet at a certain speed. The gas flow rate and wind pressure of the heating nozzle 25 are adjusted according to the first temperature detector 41, the second temperature detector 42 and the temperature monitoring device so that the profile outlet temperature is 475°C;
[0129] (3) The profile enters the quenching unit through the guide mechanism 26 at the outlet of the heat treatment device 2 for water spray cooling, so that the profile is cooled to a temperature of ≤100°C within 0.5 min;
[0130] (4) Send the cooled profile to the traction straightening machine for stretching and straightening, and the stretching amount is controlled within 0.2%;
[0131] (5) The profile after stretching and straightening is artificially aged at 120±10℃ for 20~30h to obtain an aluminum alloy profile.
[0132] Comparative Example 8
[0133] This comparative example is substantially the same as Example 8, except that after step (1), step (2) is not performed and step (3) is performed directly.
[0134] The material properties of the head, middle and tail of the profiles of Example 8 and Comparative Example 8 along the length direction were compared, and the yield rate was calculated, see Table 7 and Table 8 for details.
[0135]
[0136]
[0137] As shown in Table 7 and Table 8, for 7075 aluminum alloy, the profiles prepared by the production system of the present invention have higher strength and better consistency, and a higher yield rate. Therefore, the production system of the present invention can improve the material yield rate and reduce production costs.
[0138] The above detailed description of the present invention is intended to enable persons familiar with the art to understand the contents of the present invention and implement them, but it does not limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-strength aluminum alloy profile, characterized in that: The method comprises preparing a high-strength aluminum alloy profile using a production system, wherein the production system comprises a control module; An extruder for extruding an aluminum alloy substrate; A heat treatment device for heating a profile and controlled by a control module, comprising a support mechanism and a heating furnace and a guide mechanism arranged on the support mechanism, wherein the heating furnace comprises a furnace body, a heating nozzle, a heating assembly and a temperature monitoring device arranged on the furnace body and used to monitor the temperature of the furnace body, wherein the furnace body has a heating cavity for passing the profile and extending along the length direction of the furnace body, a cavity is formed between the inner wall of the heating cavity and the outer shell of the furnace body, the heating nozzle has a plurality of nozzles distributed on the inner wall of the heating cavity, the heating nozzle is connected to the cavity and the length and angle of the nozzle extending from the inner wall of the heating cavity are adjustable, the heating nozzle is in the shape of a corrugated tube, the heating assembly is connected to the furnace body, and comprises a heating element for heating and a heating element for generating a The heat is sent into the circulating fan of the heating cavity through the heating nozzle; the guide mechanism is used to align the profile entering the heating cavity in the up-down direction and the left-right direction, and the guide mechanism has two groups arranged at the front and rear sides of the heating furnace, each group of guide mechanisms includes a guide rail connected to the supporting mechanism and extending along the width direction of the furnace body, a first guide roller and a second guide roller slidably arranged on the guide rail, a driving member connected to the first guide roller and the second guide roller and used to drive the first guide roller and the second guide roller to move closer to or away from each other so as to align the profile located between the first guide roller and the second guide roller in the left-right direction, and a support roller connected to the supporting mechanism and parallel to the guide rail and used to align the profile located thereon in the up-down direction; Quenching module for water spray cooling of profiles; a first temperature detector for monitoring the temperature at the discharge port of the extruder; and a second temperature detector for detecting the temperature at the discharge port of the heating furnace, The preparation method comprises the following steps: (1) feeding a 6005 aluminum alloy substrate into an extrusion die of an extruder for extrusion molding to obtain a profile, wherein the temperature of the aluminum alloy substrate is 480-490° C., the heating temperature of the extrusion die is 470° C., the extrusion speed is 3 mm / s, the extrusion ratio is 30, and the profile outlet temperature is 520° C.; (2) The extruded profile is directly centered by the guide mechanism at the feed port of the heat treatment device and then enters the heating furnace, and moves from the feed port of the heating furnace to the discharge port at a certain speed, wherein the speed = extrusion speed × extrusion ratio. The gas flow rate and wind pressure of the heating nozzle are adjusted according to the temperatures measured by the first temperature detector, the second temperature detector and the temperature monitoring device so that the profile temperature at the discharge port of the heat treatment device is 550°C, and the average heating rate of the profile is 2.25°C / s; (3) The profile enters the quenching unit through the guide mechanism at the discharge port of the heat treatment device for water spray cooling, so that the profile is cooled to a temperature of ≤100°C within 0.5 min; (4) Send the cooled profile to the traction straightening machine for stretching and straightening, and the stretching amount is controlled within 0.2%; (5) The profile after stretching and straightening is artificially aged at 185℃×6h.
2. The method for preparing a high-strength aluminum alloy profile according to claim 1, characterized in that: The heating nozzles have multiple rows evenly distributed along the circumference of the heating cavity, each row of heating nozzles has multiple heating nozzles evenly arranged along the length direction of the heating cavity, and the heating nozzles in two adjacent rows are staggered.
3. The method for preparing a high-strength aluminum alloy profile according to claim 1, characterized in that: The cross section of the heating cavity perpendicular to its length direction is circular.
4. The method for preparing a high-strength aluminum alloy profile according to claim 1, characterized in that: The furnace body comprises a lower furnace body and an upper furnace body which covers the lower furnace body and is hinged to the lower furnace body. The middle areas of the upper furnace body and the lower furnace body are recessed inwards and the heating cavity is formed between the upper furnace body and the lower furnace body.
5. The method for preparing a high-strength aluminum alloy profile according to claim 1, characterized in that: The heating element is heated by electricity or natural gas.
6. The method for preparing a high-strength aluminum alloy profile according to claim 1, characterized in that: The distance between the heating nozzle and the profile is 70-90 mm.
7. The method for preparing a high-strength aluminum alloy profile according to claim 1, characterized in that: The gas flow rate of the heating nozzle is 600±20 m 3 / min, wind pressure is 900±5kPa.
Citation Information
Cited By
Aluminum material processing device capable of synchronously performing extrusion and heat treatment
CN121244720A