Alloy melting and casting ceramic material and preparation method thereof

By glueing the intermediate alloy on the ceramic intermediate, the metallurgical bond between the ceramic and the alloy matrix is ​​improved by using B and Y elements, the problem of poor bonding between the ceramic and the alloy matrix is ​​solved, and the wear resistance of alloy cast ceramic materials is significantly improved.

CN118204476BActive Publication Date: 2024-11-12TANGSHAN GUIJINJIA TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410359124.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-11-12
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Traditional wear-resistant materials have poor wear resistance under complex working conditions, and poor metallurgical bonding performance between ceramics and alloy substrates leads to insufficient wear resistance of alloy melt-cast ceramic materials.

Method used

Ceramic intermediates are used, including ZTA ceramics and intermediate alloys glued on their surface. The intermediate alloy is composed of Cu, Mg, Ti, B and Y. The mass ratio of B to Y is 6≤B/Y≤8. During bonding, Organic or inorganic adhesives are used and calcium fluoride is added to enhance metallurgical bonding and wear resistance.

Benefits of technology

The metallurgical combination of ceramics and alloy substrates is improved, and the wear resistance of alloy cast ceramic materials is significantly enhanced, which prevents ceramics from falling off, and improves the material's wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of investment casting, and proposes an alloy casting ceramic material and a preparation method thereof. The alloy casting ceramic material comprises an alloy matrix and a ceramic intermediate, and the ceramic intermediate comprises a ZTA ceramic and an intermediate alloy bonded to the surface of the ZTA ceramic; the intermediate alloy is composed of the following components in mass percentage: Cu 6% to 9%, Mg 3% to 6%, Ti 8% to 10%, B 1% to 4.5%, Y 0.2% to 0.5%, and the rest is Al and inevitable impurities. Through the above technical scheme, the problem of poor wear resistance of alloy casting ceramic materials due to poor metallurgical bonding performance between ceramics and alloy matrix in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of investment casting, and in particular to an alloy melting and casting ceramic material and a preparation method thereof. Background Art

[0002] Traditional wear-resistant materials include high-chromium cast iron alloy materials, bimetallic butt-welding materials, and metal-ceramic composite materials. These materials all have practical application technical problems such as single applicable working conditions and inability to adapt to complex working conditions. For example, the high-chromium cast iron alloy material has relatively weak erosion and wear resistance, and will quickly lose its wear resistance if it is subjected to long-term high-energy powder erosion; bimetallic butt-welding materials will produce many tiny microcracks due to differences in thermal conductivity and the breaking of chemical bonds between material crystals, and their service life will also be greatly reduced due to the generation of microcracks; metal-ceramic composite materials usually use adhesives or fasteners to connect ceramics to metal substrates, which often cause ceramics to fall off due to failure of adhesives or loose fastening, thereby reducing the wear resistance of the material.

[0003] Alloy fused-cast ceramic materials have the advantages of good wear resistance, bolt connection and easy installation, and are favored by the market. However, due to the difference in thermal expansion coefficients between ceramics and alloy matrix, it is difficult for ceramics to achieve a completely dense bond with the alloy matrix. Therefore, in order to further promote the metallurgical bonding between ceramics and alloy matrix and enhance the wear resistance of alloy fused-cast ceramic materials, it is of great significance to develop a new type of alloy fused-cast ceramic material. Summary of the invention

[0004] The present invention provides an alloy fused-cast ceramic material and a preparation method thereof, which solves the problem in the related art that the alloy fused-cast ceramic material has poor wear resistance due to poor metallurgical bonding performance between the ceramic and the alloy matrix.

[0005] The technical solution of the present invention is as follows:

[0006] The present invention provides a ceramic intermediate, comprising a ZTA ceramic and an intermediate alloy bonded to the surface of the ZTA ceramic;

[0007] The master alloy is composed of the following components in mass percentage: Cu 6%-9%, Mg 3%-6%, Ti 8%-10%, B1%-4.5%, Y 0.2%-0.5%, and the rest is Al and inevitable impurities.

[0008] As a further technical solution, the mass ratio of B to Y is 6≤B / Y≤8.

[0009] When the mass ratio of B to Y in the master alloy is 6≤B / Y≤8, it helps to further promote the metallurgical bonding of ZTA ceramics and alloy matrix during the preparation of alloy melt-cast ceramic materials, thereby further improving the wear resistance of the alloy melt-cast ceramic materials.

[0010] As a further technical solution, the bonding is carried out using an adhesive, and the adhesive includes one or both of an organic adhesive and an inorganic adhesive; the organic adhesive may be epoxy resin, phenolic resin, polyvinyl alcohol, EVA emulsion, etc., preferably phenolic resin and polyvinyl alcohol; the inorganic adhesive may be silicate, phosphate, borate, aluminate, etc., preferably silicate and borate.

[0011] As a further technical solution, during the bonding, the adhesive includes polyvinyl alcohol and sodium silicate in a mass ratio of 10 to 20:3.

[0012] As a further technical solution, the adhesive also includes calcium fluoride.

[0013] When the adhesive includes calcium fluoride, on the one hand, it can enhance the adhesive effect and prevent the ZTA ceramic from falling off during the preparation of the alloy melt-cast ceramic material; on the other hand, it can activate the ZTA ceramic and further promote the metallurgical bonding of the ZTA ceramic and the alloy matrix, thereby further improving the wear resistance of the alloy melt-cast ceramic material.

[0014] As a further technical solution, the mass ratio of calcium fluoride to adhesive is 1~5:30.

[0015] When the mass ratio of calcium fluoride to adhesive is 1-5:30, it helps to further promote the metallurgical bonding of ZTA ceramics and alloy matrix, and further improve the wear resistance of alloy melt-cast ceramic materials.

[0016] As a further technical solution, the mass ratio of the ZTA ceramic to the master alloy is 3:2~9:1.

[0017] As a further technical solution, the preparation method of the intermediate alloy is: weighing the single substance powder of each component according to the mass percentage of each component of the intermediate alloy, mixing them evenly, sintering and crushing them, and obtaining the intermediate alloy.

[0018] As a further technical solution, the mass ratio of the sum of the mass of the ZTA ceramic and the master alloy to the mass of the adhesive is 100:3-7.

[0019] The present invention also provides an alloy casting ceramic material, the raw materials of which include an alloy matrix and the ceramic intermediate.

[0020] As a further technical solution, the alloy matrix includes one of a chromium-molybdenum alloy matrix, a stainless steel alloy matrix, and a cast iron alloy matrix. The alloy matrix can be selected independently according to different working conditions. For example, for high temperature working conditions, a chromium-molybdenum alloy matrix can be selected; for easily corrosive working conditions, a stainless steel alloy matrix can be selected; for working conditions requiring vibration reduction, a cast iron alloy can be selected.

[0021] As a further technical solution, the mass ratio of the alloy matrix to the ceramic intermediate is 100~300:1.

[0022] The present invention also provides a method for preparing the alloy fused-cast ceramic material, comprising the following steps: the alloy matrix is ​​melted and then cast into a sand box containing the ceramic intermediate, and then formed to obtain the alloy fused-cast ceramic material.

[0023] The present invention also proposes the use of the alloy fused-cast ceramic material or the alloy fused-cast ceramic material prepared by the preparation method in pipelines.

[0024] The working principle and beneficial effects of the present invention are:

[0025] In the present invention, a ceramic intermediate is obtained by bonding an intermediate alloy to the surface of a ZTA ceramic, which effectively solves the problem of poor metallurgical bonding between ceramic and alloy matrix in the preparation process of alloy fused-cast ceramic materials, and improves the wear resistance of the alloy fused-cast ceramic materials. In addition, the intermediate alloy is composed of high melting point elements, low melting point elements and rare earth elements, and the wear resistance of the alloy fused-cast ceramic materials is improved by adding B and Y elements. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In the following embodiments and comparative examples, unless otherwise specified, the model of the stainless steel alloy substrate is 304 stainless steel alloy substrate; the model of the chromium-molybdenum alloy substrate is 42CrMo4; the content of chromium oxide in the ZTA ceramic is 28wt%; the model of the phenolic resin is XT-101; and the model of the polyvinyl alcohol is PVA2488.

[0028] Example 1

[0029] A method for preparing an alloy casting ceramic material comprises the following steps:

[0030] S1. Preparation of master alloy: weighing the single substance powders of each component according to the target composition of the master alloy, mixing them evenly, sintering and crushing them to obtain the master alloy;

[0031] The master alloy is composed of the following components in mass percentage: Cu 6%, Mg 3%, Ti 8%, B 1%, Y0.2%, and the rest is Al and inevitable impurities;

[0032] S2. Preparation of ceramic intermediate: After the ZTA ceramic is alkali-washed with a sodium hydroxide solution having a mass fraction of 20%, an alkali-washed ZTA ceramic is obtained, and a phenolic resin is used as an adhesive to bond the intermediate alloy to the surface of the alkali-washed ZTA ceramic to obtain a ceramic intermediate;

[0033] Among them, the mass ratio of ZTA ceramics to master alloys is 1:1, and the mass ratio of the sum of the mass of ZTA ceramics and master alloys to the mass of adhesive is 100:5;

[0034] S3. Preparation of alloy fused-cast ceramic material: the alloy matrix is ​​melted and then cast into a sand box of an inherent ceramic intermediate, formed, the casting edges and corners are removed, sandblasted, and polished to obtain the alloy fused-cast ceramic material;

[0035] Among them, the mass ratio of the chromium-molybdenum alloy matrix to the ceramic intermediate is 200:1.

[0036] Example 2

[0037] A method for preparing an alloy casting ceramic material comprises the following steps:

[0038] S1. Preparation of master alloy: weighing the single substance powders of each component according to the target composition of the master alloy, mixing them evenly, sintering and crushing them to obtain the master alloy;

[0039] The master alloy is composed of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, B 4.5%, Y0.5%, and the rest is Al and unavoidable impurities;

[0040] S2. Preparation of ceramic intermediate: After the ZTA ceramic is alkali-washed with a sodium hydroxide solution having a mass fraction of 20%, an alkali-washed ZTA ceramic is obtained, and sodium borate is used as an adhesive to bond the intermediate alloy to the surface of the alkali-washed ZTA ceramic to obtain a ceramic intermediate;

[0041] Among them, the mass ratio of ZTA ceramics to master alloys is 10:1, and the mass ratio of the sum of the mass of ZTA ceramics and master alloys to the adhesive is 100:5;

[0042] S3. Preparation of alloy fused-cast ceramic material: the alloy matrix is ​​melted and then cast into a sand box of an inherent ceramic intermediate, formed, the casting edges and corners are removed, sandblasted, and polished to obtain the alloy fused-cast ceramic material;

[0043] Among them, the mass ratio of 304 stainless steel alloy matrix to ceramic intermediate is 200:1.

[0044] Example 3

[0045] A method for preparing an alloy casting ceramic material comprises the following steps:

[0046] S1. Preparation of master alloy: weighing the single substance powders of each component according to the target composition of the master alloy, mixing them evenly, sintering and crushing them to obtain the master alloy;

[0047] The master alloy is composed of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, B 4.5%, Y0.5%, and the rest is Al and unavoidable impurities;

[0048] S2. Preparation of ceramic intermediate: After the ZTA ceramic is alkali-washed with a sodium hydroxide solution having a mass fraction of 20%, an alkali-washed ZTA ceramic is obtained, and polyvinyl alcohol and sodium silicate are used as adhesives to bond the intermediate alloy to the surface of the alkali-washed ZTA ceramic to obtain a ceramic intermediate;

[0049] The mass ratio of ZTA ceramic to master alloy is 10:1, the mass ratio of the sum of the mass of ZTA ceramic and master alloy to the adhesive is 100:5, and the mass ratio of polyvinyl alcohol to sodium silicate in the adhesive is 15:3.

[0050] S3. Preparation of alloy fused-cast ceramic material: the alloy matrix is ​​melted and then cast into a sand box of an inherent ceramic intermediate, formed, the casting edges and corners are removed, sandblasted, and polished to obtain the alloy fused-cast ceramic material;

[0051] Among them, the mass ratio of 304 stainless steel alloy matrix to ceramic intermediate is 200:1.

[0052] Example 4

[0053] The difference between this embodiment and embodiment 3 is that, in this embodiment, the master alloy is composed of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, B 2.5%, Y 0.5%, and the rest is Al and unavoidable impurities.

[0054] Example 5

[0055] The difference between this embodiment and embodiment 3 is that, in this embodiment, the master alloy is composed of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, B 3%, Y 0.5%, and the rest is Al and inevitable impurities.

[0056] Example 6

[0057] The difference between this embodiment and embodiment 3 is that, in this embodiment, the master alloy is composed of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, B 4%, Y 0.5%, and the rest is Al and unavoidable impurities.

[0058] Example 7

[0059] The only difference between this embodiment and embodiment 6 is that in this embodiment, the adhesive includes polyvinyl alcohol, sodium silicate and calcium fluoride, the mass ratio of polyvinyl alcohol to sodium silicate in the adhesive is 15:3, and the mass ratio of calcium fluoride to the adhesive is 1:40.

[0060] Example 8

[0061] The only difference between this embodiment and embodiment 7 is that in this embodiment, the mass ratio of polyvinyl alcohol to sodium silicate in the adhesive is 15:3, and the mass ratio of calcium fluoride to the adhesive is 7:30.

[0062] Example 9

[0063] The only difference between this embodiment and embodiment 7 is that in this embodiment, the mass ratio of polyvinyl alcohol to sodium silicate in the adhesive is 15:3, and the mass ratio of calcium fluoride to the adhesive is 1:30.

[0064] Example 10

[0065] The only difference between this embodiment and embodiment 7 is that in this embodiment, the mass ratio of polyvinyl alcohol to sodium silicate in the adhesive is 15:3, and the mass ratio of calcium fluoride to the adhesive is 5:30.

[0066] Comparative Example 1

[0067] The difference between this comparative example and Example 2 is that in this comparative example, the master alloy consists of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, B 5%, and the rest is Al and inevitable impurities.

[0068] Comparative Example 2

[0069] The difference between this comparative example and Example 2 is that in this comparative example, the master alloy consists of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, Y 5%, and the rest is Al and inevitable impurities.

[0070] Comparative Example 3

[0071] The difference between this comparative example and Example 2 is that in this comparative example, the master alloy consists of the following components in mass percentage: Cu 9%, Mg 6%, Ti 10%, and the rest is Al and inevitable impurities.

[0072] The alloy melt-cast ceramic materials prepared in Examples 1 to 10 and Comparative Examples 1 to 3 were subjected to the following performance tests:

[0073] ① Brinell hardness: Test the Brinell hardness of alloy cast ceramic materials in accordance with GB / T 231.1-2018 "Brinell hardness test for metallic materials - Part 1: Test method";

[0074] ② Wear weight loss: In the wear weight loss test, the wear testing machine model is MLD-10, the lower sample is silicon nitride, the rotation speed is 200r / min, the average particle size of quartz sand is 50 mesh, the entire test is carried out under 2J impact energy, the test time is 240min, each cycle is 30min, and the wear weight loss during the entire test process is measured.

[0075] The performance test results are shown in Table 1 below.

[0076] Table 1 Performance test results

[0077]

[0078] Comparison between Example 2 and Comparative Examples 1 to 3 shows that by adding B and Y elements to the intermediate alloy, the wear resistance of the alloy casting ceramic material is improved. Comparison between Examples 3 to 4 and Examples 5 to 6 shows that when the mass ratio of B to Y in the intermediate alloy is 6≤B / Y≤8, it helps to further improve the wear resistance of the alloy casting ceramic material. Comparison between Example 6 and Examples 7 to 10 shows that when the adhesive includes calcium fluoride, the wear resistance of the alloy casting ceramic material can be further improved. Comparison between Examples 9 to 10 and Examples 7 to 8 shows that when the mass ratio of calcium fluoride to adhesive is 1 to 5:30, it helps to further improve the wear resistance of the alloy casting ceramic material.

[0079] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A ceramic intermediate, It is characterized in that It includes ZTA ceramic and a master alloy bonded to the surface of the ZTA ceramic; The master alloy is composed of the following components in mass percentage: Cu 6%-9%, Mg 3%-6%, Ti 8%-10%, B 1%-4.5%, Y 0.2%-0.5%, and the rest is Al and inevitable impurities.

2. A ceramic intermediate according to claim 1, It is characterized in that The mass ratio of B to Y is 6≤B / Y≤8.

3. A ceramic intermediate according to claim 1, It is characterized in that During the bonding, the adhesive comprises polyvinyl alcohol and sodium silicate in a mass ratio of 10 to 20:

3.

4. A ceramic intermediate according to claim 3, It is characterized in that The adhesive also includes calcium fluoride.

5. A ceramic intermediate according to claim 4, It is characterized in that The mass ratio of calcium fluoride to adhesive is 1-5:

30.

6. A ceramic intermediate according to claim 1, It is characterized in that The mass ratio of the ZTA ceramic to the master alloy is 3:2-9:

1.

7. An alloy casting ceramic material, It is characterized in that The raw materials include an alloy matrix and a ceramic intermediate according to any one of claims 1 to 6.

8. The alloy casting ceramic material according to claim 7, It is characterized in that The alloy matrix includes one of a chromium-molybdenum alloy matrix, a stainless steel alloy matrix, and a cast iron alloy matrix.

9. A method for preparing the alloy melt-cast ceramic material according to any one of claims 7 to 8, It is characterized in that The following steps are involved: The alloy matrix is ​​melted and cast into a sand box containing the ceramic intermediate to form an alloy melt-cast ceramic material.

10. Use of the alloy-cast ceramic material according to any one of claims 7 to 8 or the alloy-cast ceramic material prepared by the preparation method according to claim 9 in pipelines.

Citation Information

Patent Citations

  • Preparation method of ceramic particle reinforced steel-based composite material based on SHS technology

    CN111730042A

  • NiCrAl modified oxide ceramic reinforced iron-based composite material as well as preparation method and application thereof

    CN111809099A

  • Wear-resistant metal-ceramic composite material with long service life and preparation method thereof

    CN112207273A

  • Method for preparing ZTA ceramic particle reinforced high-chromium cast iron-based wear-resistant composite material

    CN113560540A

  • Metal-ceramic composites

    US5217816A