A method for thickening metal after SiC ohmic contact

By forming a protective layer on the metal layer in the SiC device and removing part of the protective layer, the problem of weak adhesion caused by the roughness and oxidation of the Ni alloy layer is solved, the risk of deformation is reduced, and the electrical performance and production efficiency of the SiC device are improved.

CN118280824BActive Publication Date: 2024-10-01WUXI CHAAO MICROELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410712235.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

In SiC devices, the roughness and oxidation of the Ni alloy layer results in weak adhesion and easy falling off during the metal thickening process, affecting electrical performance and reliability. The existing wet etching removal process is unstable and difficult to effectively solve these problems.

Method used

After making a metal layer on the SiC wafer, a protective layer is formed, and the remaining protective layer is formed by removing part of the protective layer, and then the metal layer is thickened on top, and the relationship between the thickness and expansion rate of each layer is controlled to ensure that the protective layer does not affect Adhesion and electrical properties of thickened metal layers.

Benefits of technology

Through this method, the risk of deformation of SiC devices during the production of thickened metal layers is reduced, the production efficiency and electrical performance stability are improved, and the thermal conductivity, electromagnetic shielding and mechanical strength of the device are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118280824B_ABST
    Figure CN118280824B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for thickening metal after SiC ohmic contact, comprising the following steps: step S100: making a metal layer on the front or back of a SiC wafer, and forming an ohmic contact after annealing; step S200: making a protective layer on the metal layer; step S300: removing at least part of the protective layer to form a remaining protective layer; step S400: making a thickened metal layer on the remaining protective layer. The present invention provides a protective layer outside the metal layer, so that the metal layer can be protected from the influence of other subsequent processes in the subsequent process, and even if the protective layer is oxidized, the protective layer can be etched away by wet etching or dry etching, and the removal process of the oxidized part of the protective layer is highly controllable and stable, and will not affect the adhesion effect of the subsequent thickened metal layer, thereby reducing the damage to the electrical properties of the SiC device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of SiC ohmic contact metal thickening, and more specifically, to a method for SiC ohmic contact back metal thickening. Background Art

[0002] SiC (Silicon Carbide) is one of the wide bandgap semiconductor materials that has developed rapidly in the past decade. Compared with the widely used semiconductor materials Si, Ge and GaAs, SiC material has many advantages such as wide bandgap, high breakdown electric field, high carrier saturation drift rate, high thermal conductivity, high power density, etc. It is an ideal material for preparing high-temperature, high-power and high-frequency devices. Low specific contact resistance and high stability are two important factors that determine the performance of SiC devices. Therefore, in order to give full play to the performance advantages of SiC devices, the production process of ohmic contacts and electrodes in the SiC device manufacturing process plays a very important role.

[0003] At present, Ni (nickel) alloy is usually used as ohmic contact metal in SiC (silicon carbide) devices. After Ni alloy is deposited on the surface of SiC wafer, it is annealed at a high temperature of up to 1000 degrees C to form a good ohmic contact. However, due to the Ni alloy and other subsequent process, the Ni alloy layer is prone to roughness, oxidation and other undesirable appearances, and it is not easy to remove. In the subsequent metal thickening process, the thickened metal layer is not firmly adhered, the thickened metal layer falls off, and the ohmic contact layer is deformed, which damages the electrical performance of the SiC device and creates reliability risks.

[0004] In response to these problems, the conventional solution is to wet-etch the Ni alloy layer, which has two main disadvantages: (1) The Ni alloy layer is relatively loose and easily oxidized, and wet etching cannot effectively remove the oxidized part of the Ni alloy layer; (2) The oxidized part of the Ni alloy layer has poor consistency, which makes the removal process difficult to control. The unstable removal process will affect the contact effect of the ohmic contact or the adhesion effect or deformation of the subsequent thickened metal layer, which will damage the electrical performance of the SiC device and create reliability risks. Therefore, it is very important to develop a new SiC metal thickening process. Summary of the invention

[0005] Based on this, the present invention provides a method for thickening metal after SiC ohmic contact, aiming to partially or completely solve the above technical problems. The present invention is achieved through the following technical solutions:

[0006] A method for thickening metal after SiC ohmic contact, comprising the following steps:

[0007] Step S100: forming a metal layer on the front or back side of the SiC wafer and forming an ohmic contact after annealing;

[0008] Step S200: fabricate a protective layer on the metal layer;

[0009] Step S300: remove at least part of the protective layer to form a remaining protective layer;

[0010] Step S400: fabricate a thickened metal layer on the remaining protective layer;

[0011] Wherein, the thickness relationship of the metal layer, the remaining protective layer, and the thickened metal layer satisfies:

[0012] P = P1 + P2, 1.0 ≤ P ≤ 8.0;

[0013] P1 = λ1 (E1 × D1) / (E × D4) + λ2 (E2 × D3) / (E × D4);

[0014] P2 = λ3 (E1 × D1) / (E2 × D3);

[0015] Wherein, P is the total deformation, P1 is the first deformation, and P2 is the second deformation;

[0016] D1 is the thickness of the metal layer, E1 is the linear expansion rate of the metal layer, λ1 is the first deformation adjustment coefficient, related to the linear expansion rates of the metal layer and the thickened metal layer; D3 is the thickness of the remaining protective layer, E2 is the linear expansion rate of the remaining protective layer, λ2 is the second deformation adjustment coefficient, related to the linear expansion rates of the remaining protective layer and the thickened metal layer; D4 is the thickness of the thickened metal layer; E is the linear expansion rate of the thickened metal layer, and λ3 is the third deformation adjustment coefficient, related to the linear expansion rates of the metal layer and the remaining protective layer.

[0017] Optionally, in step S200, the thickness of the fabricated protective layer is D2, satisfying: A1 ≤ D2 / D1 ≤ A2, 0.25 ≤ A1 ≤ 0.4, 0.5 ≤ A2 ≤ 5.0, 0 < D3 / D2 ≤ A3, D1 + D3 ≤ D4, 0 < A3 ≤ 0.5, and A1, A2, and A3 are all set constants.

[0018] Optionally, the protective layer includes a first film layer and a second film layer. The thickness of the first film layer is D21, and the thickness of the second film layer is D22, satisfying: the sum of D21 and D22 is equal to D2. The first film layer connects the metal layer and the second film layer, satisfying: D21 = D3, D22 / D1 ≤ A4, 0.1 ≤ A4 ≤ 0.8, and A4 is a set constant.

[0019] Optionally, the numerical range of the thickness D1 of the metal layer is: greater than or equal to 50nm and less than or equal to 600nm, the numerical range of the thickness D2 of the protective layer is: greater than or equal to 10nm and less than or equal to 2000nm; the numerical range of the thickness D3 of the remaining protective layer is: greater than 0 and less than or equal to 1000nm; the numerical range of the thickness D4 of the thickened metal layer is: greater than 50nm and less than or equal to 6000nm.

[0020] Optionally, in step S100, a layer of Ni alloy is deposited on the back or front side of the SiC wafer, and annealed to form a Ni alloy layer with a thickness of D1, and the Ni alloy layer with a thickness of D1 is used as a metal layer to complete the ohmic contact production of SiC.

[0021] Optionally, in the step S100, the deposition temperature T1 is 25 degrees to 400 degrees, the annealing time S1 is 5 minutes to 15 minutes, and the deposition method is evaporation or sputtering.

[0022] Optionally, in the step S200, the protective layer with a thickness of D2 is deposited on the metal layer, the deposition temperature T2 is 25 degrees to 400 degrees, and the deposition method is: evaporation or sputtering.

[0023] Optionally, in the step S200, the protective layer is a metal protective film, and the metal includes Al, Ti, and TiAl alloy.

[0024] Optionally, in the step S300, at least a portion of the protective layer is wet-etched or dry-etched to form the remaining protective layer with a thickness of D3.

[0025] Optionally, in the step S400, the thickened metal layer with a thickness of D4 is deposited on the remaining protective layer, the deposition temperature T3 is 25 degrees to 400 degrees, and the deposition method is: evaporation, sputtering, and electroplating.

[0026] Beneficial technical effects of the present invention:

[0027] (1)For the thickness D1 of the metal layer, the thickness D2 of the protective layer, the thickness D3 of the remaining protective layer, and the thickness D4 of the thickened metal layer in the SiC device as a whole, the following conditions are satisfied: A1 ≤ D2 / D1 ≤ A2, 0.25 ≤ A1 ≤ 0.4, 0.6 ≤ A2 ≤ 5.0, 0 < D3 / D2 ≤ A3, D1 + D3 ≤ D4, 0 < A3 ≤ 0.5, D21 = D3, D22 / D1 ≤ A4, 0.1 ≤ A4 ≤ 0.8. A1, A2, A3, and A4 are set constants, which can prevent the protective layer from being too thin to play a protective role and can also avoid, as much as possible, the increase in deposition time due to the excessive thickness of the protective layer. An excessive thickness of the protective layer will also affect the time for removing the protective layer. In this way, the time for removing the protective layer can be reduced as a whole, and at the same time, the production of the thickened metal layer is ensured, improving the yield and production efficiency of the SiC ohmic contact and the production of the thickened metal layer.

[0028] (2)On the basis that the SiC device satisfies the above conditions, the relationship between the metal layer, the remaining protective layer, and the thickened metal layer of the SiC device as a whole also satisfies: P = P1 + P2, 1.0 ≤ P ≤ 8.0, P1 = λ1(E1×D1) / (E×D4) + λ2(E2×D3) / (E×D4), P2 = λ3(E1×D1) / (E2×D3). Thus, the shrinkage of the SiC device or the risk of deformation or deformation that may occur in subsequent processes such as cutting and grooving can be reduced, and the risk of deformation or the amount of deformation of the metal layer, the remaining protective layer, and the thickened metal layer of the SiC device as a whole can be reduced, and the heat conduction, electromagnetic shielding, and overall mechanical strength of the SiC device are ensured.

[0029] (3)A protective layer is provided outside the metal layer, which can protect the metal layer from the influence of subsequent other processes during the subsequent process. Moreover, even after the protective layer is oxidized, the protective layer can be removed by wet etching or dry etching. The removal process of the oxidized part of the protective layer has strong controllability and good stability, and the removal process will not affect the contact effect of the completed ohmic contact and the adhesion effect of the subsequent thickened metal layer, reducing the damage to the electrical performance of the SiC device. Description of the Drawings

[0030] Figure 1 is a schematic structural diagram after SiC ohmic contact in the method for metal thickening after SiC ohmic contact of the present invention application;

[0031] Figure 2 is a schematic structural diagram for fabricating a protective layer after SiC ohmic contact in the method for metal thickening after SiC ohmic contact of the present invention application;

[0032] Figure 3 is a schematic structural diagram for forming a remaining protective layer by removing part of the protective layer after SiC ohmic contact in the method for metal thickening after SiC ohmic contact of the present invention application;

[0033] Figure 4 It is a structural schematic diagram of the method for thickening metal after SiC ohmic contact applied by the present invention, in which a part of the protective layer is removed after SiC ohmic contact to form a remaining protective layer and then the thickened metal layer is produced.

[0034] Figure 5 It is a schematic diagram of the structure of the protective layer in the method for thickening the metal after SiC ohmic contact applied by the present invention. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure more clear, the embodiments of the present disclosure are further described in detail below in conjunction with the accompanying drawings and embodiments; it should be understood that the specific embodiments described herein are only used to explain the embodiments of the present disclosure and are not used to limit the embodiments of the present disclosure;

[0036] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no substantial technical significance. Any structural modification, change in proportion relationship or adjustment in size, without affecting the effects and purposes that can be produced by the present invention, should still fall within the scope of the technical contents disclosed by the present invention; at the same time, the terms such as "and" and "or" quoted in this specification are only for the convenience of description, and are not used to limit the scope of implementation. The change or adjustment of their relative relationship should also be regarded as the scope of implementation of the present invention without substantially changing the technical contents; in addition, the various embodiments of the present invention are not independent of each other, but can be combined;

[0037] The terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features; thus, the features defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features; in the description of the present invention application, unless otherwise specified, "plurality" means two or more;

[0038] like Figure 1-Figure 5 As shown, the present invention provides a method for thickening metal after SiC ohmic contact, comprising the following steps:

[0039] Step S100: forming a metal layer 20 on the front or back side of the SiC wafer 10, and forming an ohmic contact after annealing;

[0040] In some embodiments, a layer of Ni alloy is deposited on the back or front side of the SiC wafer, and annealed to form a Ni alloy layer with a thickness of D1, and the Ni alloy layer with a thickness of D1 is used as the metal layer 20 to complete the ohmic contact of SiC;

[0041] Specifically, the deposition temperature T1 is 25 degrees to 400 degrees, the annealing time S1 is 5 minutes to 15 minutes, the deposition method is evaporation or sputtering, and the value range of the thickness D1 is greater than or equal to 50 nm and less than or equal to 600 nm.

[0042] The deposition temperature T1 is 25 degrees-400 degrees, and the value can be 25 degrees, 30 degrees, 40 degrees, 50 degrees, 60 degrees, 70 degrees, 80 degrees, 90 degrees, 100 degrees, 150 degrees, 200 degrees, 250 degrees, 300 degrees, 350 degrees, 400 degrees, or a numerical range between any two of the above values. The technicians can set it according to actual conditions, and this application does not make any settings for this.

[0043] The annealing time S1 is 5min-15min, and the value can be 5min, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min, 15min, or a numerical range between any two of the above values. The technicians can set it according to the actual situation, and this application does not make any settings for this.

[0044] The value of thickness D1 can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, or it can be a numerical range between any two of the above values. The technicians can set it according to the actual situation, and this application does not make any settings for this.

[0045] In this way, the ohmic contact of SiC can be well completed by setting the deposition temperature T1, annealing time S1 and Ni alloy layer thickness D1, thus forming a better ohmic contact.

[0046] Preferably, the deposition temperature T1 is 400 degrees, the annealing time is 8min-10min, and the Ni alloy with a thickness of 100nm-120nm is rapidly annealed at 1000 degrees. The Ni alloy does not completely react with SiC, and the Ni alloy on the surface that does not react with SiC is still relatively dense, which can prevent carbon precipitation. At this time, no black carbon precipitation can be observed or detected on the back or front side of the SiC wafer 10.

[0047] Step S200: forming a protective layer 30 on the metal layer 20;

[0048] In some embodiments, a protection layer 30 with a thickness D2 is deposited on the metal layer 20 .

[0049] Specifically, the deposition temperature T2 is 25 degrees to 400 degrees, the deposition method is evaporation or sputtering, and the thickness D2 has a value range of greater than or equal to 10 nm and less than or equal to 2000 nm.

[0050] The deposition temperature T2 is 25 degrees-400 degrees, and the value can be 25 degrees, 50 degrees, 75 degrees, 100 degrees, 125 degrees, 150 degrees, 175 degrees, 200 degrees, 250 degrees, 300 degrees, 350 degrees, 400 degrees, or a numerical range between any two of the above values. The technicians can set it according to actual conditions, and this application does not make any settings for this.

[0051] The value of thickness D2 can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm, or it can be a numerical range between the above values. The technicians can set it according to the actual situation, and this application does not make any settings for this.

[0052] In some embodiments, any protective layer can be considered. For example, the protective layer 30 uses a metal protective film, and the metal includes Al, Ti, TiAl alloy, etc., which is an Al film, a Ti film, a TiAl alloy film, etc., so that the influence of the later process on the metal protective film can be avoided and the stability of the metal protective film can be ensured. Of course, it can also be other metals, and technicians can set it according to actual conditions. This application does not make any settings for this.

[0053] In some embodiments, Figure 4 As shown, the thickness D2 of the protective layer 30 and the thickness D1 of the metal layer satisfy: A1≤D2 / D1≤A2, 0.25≤A1≤0.4, 0.5≤A2≤5.0, A1 and A2 are both set constants. Specifically, the set constant A1 can be 0.25, 0.3, 0.4, and the set constant A2 can be 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0. The technicians can set the set constants A1 and A2 according to the actual situation, and this application does not make any settings for this.

[0054] The relationship between the thickness D2 of the protective layer and the thickness D1 of the metal layer can prevent the protective layer 30 from being too thin to play a protective role, prevent the protective layer 30 from being too thick to increase the deposition time, and prevent the protective layer 30 from being too thick to affect the subsequent removal of the protective layer to form the remaining protective layer 40, thereby affecting the overall yield and production efficiency of SiC ohmic contact and thickened metal layer production.

[0055] In some embodiments, Figure 5 As shown, the protective layer 30 includes a first film layer 31 and a second film layer 32. The thickness of the first film layer is D21, and the thickness of the second film layer is D22, satisfying: the sum of D21 and D22 is equal to D2, and the first film layer 31 connects the metal layer 31 and the second film layer 32.

[0056] In some embodiments, the first film layer 31 is deposited at a temperature of 25 degrees to 400 degrees, and the deposition method is evaporation or sputtering. The thickness of the first film layer 31 after deposition is D21. Similarly, the second film layer 32 is deposited at a temperature of 25 degrees to 400 degrees, and the deposition method is evaporation or sputtering. The thickness of the second film layer 32 after deposition is D22.

[0057] In some embodiments, the following conditions are satisfied: D21=D3, D22 / D1≤A4, 0.1≤A4≤0.8, and A4 is a set constant. This can prevent the first film layer 31 from being too thin, so as to ensure that the first film layer 31 can play an antioxidant protection role. It can also prevent the second film layer 32 from being too thick, and can appropriately reduce the time for removing at least part of the protective layer to ensure the production of the thickened metal layer 50. In this way, the needs of antioxidant protection and removal of at least part of the protective layer can be met at the same time, that is, the first film layer 31 with a thickness of D21 plays an antioxidant protection role (corresponding to when D21 is equal to D3), and when removing at least part of the protective layer, the second film layer 32 with a thickness of D22 can be directly removed. Overall, the time for removing part of the protective layer can be reduced, and the production of the thickened metal layer 50 can be more conveniently ensured, thereby appropriately improving the production efficiency of SiC ohmic contacts and thickened metal layers.

[0058] Step S300: removing at least part of the protective layer to form a remaining protective layer 40;

[0059] In some embodiments, at least a portion of the protection layer may be wet etched or dry etched away.

[0060] In some embodiments, at least a portion of the protective layer is removed to form a remaining protective layer 40 with a thickness of D3, and the numerical range of the thickness D3 is: greater than or equal to 0 and less than or equal to 1000nm. Specifically, the value of the thickness D3 can be 0nm, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, or a numerical range between the above values. The technician can set it according to the actual situation, and this application does not make any settings for this. In this way, the above-mentioned wet etching or dry etching of at least a portion of the protective layer can be used for the subsequent production of a thickened metal layer to ensure the overall size requirements of the entire SiC device.

[0061] Step S400 : forming a thickened metal layer 50 on the remaining protective layer 40 .

[0062] In some embodiments, the thickened metal layer 50 formed by thickening the metal can be used to protect the metal layer, can also be used to protect the remaining protective layer, can also be used to increase the thermal conductivity (such as heat dissipation performance) and electromagnetic shielding performance of the SiC device, and can also be used to provide additional or overall structural support for the SiC device, thereby increasing the overall (such as mechanical) structural strength of the SiC device.

[0063] In some embodiments, any thickening process and thickening metal layer can be considered. For example, the thickening metal layer can be thickened by deposition, sputtering, electroplating and other processes. The thickened metal layer includes Au, Ag, NiAu, NiAg, TiNiAu, TiNiAg, and the technicians can reasonably set it according to the actual situation. The embodiment of the present application does not set it.

[0064] In some embodiments, the deposition temperature T3 is 25-400 degrees, the deposition method is evaporation, sputtering, electroplating, and the thickness D4 has a value range of greater than 50 nm and less than or equal to 6000 nm.

[0065] The deposition temperature T3 is 25 degrees-400 degrees, and the value can be 25 degrees, 30 degrees, 40 degrees, 50 degrees, 60 degrees, 70 degrees, 80 degrees, 90 degrees, 100 degrees, 150 degrees, 200 degrees, 250 degrees, 300 degrees, 350 degrees, 400 degrees, or a numerical range between any two of the above values. The technicians can set it according to actual conditions, and this application does not make any settings for this.

[0066] The value of the thickness D4 can be 51nm, 60nm, 80nm, 100nm, 1000nm, 1500nm, 2000nm, 2500nm, 3000nm, 3500nm, 4000nm, 4500nm, 5000nm, 5500nm, 6000nm, or can be the value range between any two of the above values. Those skilled in the art can set it according to the actual situation, and this application does not make settings on this.

[0067] In some embodiments, as Figure 4 shown, the thickness D2 of the protective layer, the thickness D1 of the metal layer, the thickness D3 of the remaining protective layer 40, and the thickness of the thickened metal layer satisfy: 0 < D3 / D2 ≤ A3, D1 + D3 ≤ D4, 0 < A3 ≤ 0.5. Obviously, when D3 is not equal to 0, this can reduce the time for removing at least part of the protective layer, and at the same time ensure the production of the thickened metal layer 50, and can also avoid the over-thick protective layer 30 increasing the deposition time, thereby affecting the yield and production efficiency of the SiC ohmic contact and the production of the thickened metal layer as a whole.

[0068] However, on the basis of forming the remaining protective layer 40, in the subsequent thickening process of the thickened metal layer 50, the metal layer 20 is located on the upper side of the remaining protective layer 40, and the thickened metal layer 50 is located on the lower side of the remaining protective layer 40. Under the deposition temperature and deposition method in the thickening process of the thickened metal layer 50, after the deposition temperature (which can mean heating to a high temperature) is cooled, and even during the subsequent processes such as dicing or laser grooving and cutting of the SiC wafer, the material, thickness, area, and expansion coefficient of the metal layer 20 are different from those of the thickened metal layer 50, which may cause the risk of deformation or deformation of the SiC device. Exemplarily, there are partial gaps between at least two of the metal layer 20, the remaining protective layer 40, and the thickened metal layer 50, or there are cracks in the whole SiC device. This will also reduce the electromagnetic shielding and overall mechanical strength of the SiC device. Therefore, it is necessary to reasonably set the thickness, area, etc. of the thickened metal layer 50 to reduce or avoid the risk of deformation or deformation of the SiC device.

[0069] In some embodiments, in a SiC device, if the thickness D1 of the metal layer 20 is too large, when the SiC device is subjected to heating and then cooling, wheel cutting or laser grooving, cutting and other processing, the thermal expansion of the metal layer 20, if the thickness D1 of the metal layer 20 is greater than the thickness D4 of the thickened metal layer 50, the influence of the thermal expansion of the metal layer 20 becomes greater, thereby causing deformation, which may cause cracks or cracks in the remaining protective layer 30, affecting the ohmic contact effect of the SiC device. Accordingly, it is necessary to set the thickness D4 of the thickened metal layer 50 to be greater than or equal to the sum of the thickness D1 of the metal layer 20 and the thickness D3 of the remaining protective layer 40, so that the difference in the tensile stress between the front and back sides of the thickened metal layer 50 along the vertical direction from the thickened metal layer 50 to the metal layer 20 becomes the main deformation factor, thereby reducing the possible deformation risk of the metal layer 20 and the remaining protective layer 40 or the influence of deformation on the metal layer 20 or the thickened metal layer 50.

[0070] In some embodiments, in the metal layer 20, the remaining protective layer 40 and the thickened metal layer 50 of the SiC device, the range of the thickness D1 of the metal layer 20 is: greater than or equal to 50nm and less than or equal to 600nm, and the thickness D4 of the thickened metal layer 50 is formed to be greater than the sum of the thicknesses D1 and D3, and the value range of the thickness D4 is formed to be: greater than 50nm and less than or equal to 6000nm. Further, considering the risk of deformation and the influence of deformation, the total deformation amount P is set accordingly, and the total deformation amount P can be used to adjust the relationship between the metal layer 20, the remaining protective layer 40 and the thickened metal layer 50, and make the relationship between the metal layer 20, the remaining protective layer 40 and the thickened metal layer 50 satisfy:

[0071] P1=λ1(E1×D1) / (E×D4)+λ2(E2×D3) / (E×D4)

[0072] P2=λ3(E1×D1) / (E2×D3)

[0073] P = P1 + P2, 1.0 ≤ P ≤ 8.0;

[0074] Among them, P is the total deformation, P1 is the first deformation, and P2 is the second deformation;

[0075] Among them, E1 is the linear expansion coefficient of the metal layer, λ1 is the first deformation adjustment coefficient, which is related to the linear expansion coefficient of the metal layer and the thickened metal layer; E2 is the linear expansion coefficient of the remaining protective layer, λ2 is the second deformation adjustment coefficient, which is related to the linear expansion coefficient of the remaining protective layer and the thickened metal layer; E is the linear expansion coefficient of the thickened metal layer, λ3 is the third deformation adjustment coefficient, which is related to the linear expansion coefficient of the metal layer and the remaining protective layer.

[0076] In some embodiments, the second deformation amount P2 is relatively small compared to P1, and the first deformation amount P1 is relatively large. Correspondingly, the total deformation amount P can also be set equal to P1. Of course, the actual deformation amounts of P1 and P2 can also be compared and analyzed, and other calculation methods can be adopted. For example, the total deformation ratio Q is calculated. Exemplarily, Q = (P1 + P2) / (P1 - P2), and 1.0 < Q ≤ 5.0. At the same time, it should be noted that the above λ1, λ2, and λ3 can also be theoretical calculation and analysis parameters or empirical parameters. Exemplarily, the value range of the above λ1 is from 0.3 to 3.0, the value range of λ2 is from 0.3 to 3.0, and the value range of λ3 is from 0.1 to 5.0. Of course, the specific values of λ1, λ2, and λ3 can be reasonably set according to the actual situation, and this application does not limit this.

[0077] In some other embodiments, considering that subsequent SiC devices usually undergo processes such as dicing wheel cutting or laser grooving and cutting, the above calculation method can also be appropriately adjusted. E1 is the bending strength of the metal layer 20, λ1 is the first deformation adjustment coefficient, which is related to the bending strengths of the metal layer 20 and the thickened metal layer 50; E2 is the bending strength of the remaining protective layer 40, λ2 is the second deformation adjustment coefficient, which is related to the bending strengths of the remaining protective layer 40 and the thickened metal layer 50, E is the bending strength of the thickened metal layer 50, λ3 is the third deformation adjustment coefficient, which is related to the bending strengths of the metal layer 20 and the remaining protective layer 40, and the corresponding range of the total deformation amount P can also be 1.0 ≤ P ≤ 8.0.

[0078] In some embodiments, the total deformation amount P can be 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 6.5, 7.0, 7.5, 8.0, and the total deformation ratio Q can be 1.0, 2.0, 3.0, 4.0, 5.0. Preferably, 1.0 ≤ P ≤ 5.0, and it can also be the numerical range between any two of the above values. Those skilled in the art can set the numerical values or ranges of P and Q according to the actual situation, and this application does not set this.

[0079] In this application, when facing the heating and cooling of SiC wafers, dicing wheel cutting or laser grooving and cutting processes, by setting the total deformation amount P, the relative deformation amounts between the metal layer 20, the remaining protective layer 40, and the thickened metal layer 50 can be adjusted, thereby reducing or minimizing the risk or the amount of deformation of the overall deformation of the metal layer, the remaining protective layer, and the thickened metal layer of the SiC device, and also ensuring the heat conduction, electromagnetic shielding, and overall mechanical strength of the SiC device.

[0080] At the same time, by providing a protective layer outside the metal layer, the metal layer can be protected from being affected by other subsequent process steps during the subsequent process steps. Even after the protective layer is oxidized, the protective layer can be etched away by wet etching or dry etching. The removal process of the oxidized portion of the protective layer is highly controllable and has good stability. The removal process will not affect the contact effect of the completed ohmic contact and the adhesion effect of the subsequent thickened metal layer, thereby reducing or minimizing the risk of overall deformation of the metal layer, the remaining protective layer and the thickened metal layer of the SiC device or the amount of deformation, thereby ensuring the thermal conduction, electromagnetic shielding and overall mechanical strength of the SiC device and reducing damage to the electrical properties of the SiC device.

[0081] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0082] Those skilled in the art can understand that the steps, measures, and schemes in the various operations, methods, and processes discussed in the present application can be alternated, changed, combined, or deleted; further, other steps, measures, and schemes in the various operations, methods, and processes discussed in the present application can also be alternated, changed, rearranged, decomposed, combined, or deleted; further, the steps, measures, and schemes in the various operations, methods, and processes disclosed in the present application in the prior art can also be alternated, changed, rearranged, decomposed, combined, or deleted;

[0083] The above-described embodiments only express several implementation methods of the embodiments of the present disclosure, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the patent scope of the embodiments of the present disclosure. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the embodiments of the present disclosure, which all belong to the protection scope of the embodiments of the present disclosure. Therefore, the protection scope of the embodiments of the present disclosure shall be based on the attached claims.

Claims

1. A method for thickening metal after SiC ohmic contact, characterized in that: It includes the following steps: Step S100: Fabricate a metal layer on the front or back of the SiC wafer, and form an ohmic contact after annealing; Step S200: Fabricate a protective layer on the metal layer; Step S300: Remove at least part of the protective layer to form a remaining protective layer; Step S400: Fabricate a thickened metal layer on the remaining protective layer; Wherein, the thickness relationship of the metal layer, the remaining protective layer, and the thickened metal layer satisfies: P = P1 + P2, 1.0 ≤ P ≤ 8.0; P1 = λ1 (E1 × D1) / (E × D4) + λ2 (E2 × D3) / (E × D4); P2 = λ3 (E1 × D1) / (E2 × D3); Wherein, P is the total deformation, P1 is the first deformation, and P2 is the second deformation; D1 is the thickness of the metal layer, E1 is the linear expansion rate of the metal layer, λ1 is the first deformation adjustment coefficient, which is related to the linear expansion rates of the metal layer and the thickened metal layer; D3 is the thickness of the remaining protective layer, E2 is the linear expansion rate of the remaining protective layer, λ2 is the second deformation adjustment coefficient, which is related to the linear expansion rates of the remaining protective layer and the thickened metal layer; D4 is the thickness of the thickened metal layer; E is the linear expansion rate of the thickened metal layer, and λ3 is the third deformation adjustment coefficient, which is related to the linear expansion rates of the metal layer and the remaining protective layer.

2. The method for thickening SiC ohmic contact metal after claim 1, characterized in that: In step S200, the thickness of the fabricated protective layer is D2, satisfying: A1 ≤ D2 / D1 ≤ A2, 0.25 ≤ A1 ≤ 0.4, 0.5 ≤ A2 ≤ 5.0, 0 < D3 / D2 ≤ A3, D1 + D3 ≤ D4, 0 < A3 ≤ 0.5, and A1, A2, and A3 are all set constants.

3. The method for thickening SiC ohmic contact metal after claim 2, characterized in that: The protective layer includes a first film layer and a second film layer. The thickness of the first film layer is D21, and the thickness of the second film layer is D22, satisfying: the sum of D21 and D22 is equal to D2. The first film layer connects the metal layer and the second film layer, satisfying: D21 = D3, D22 / D1 ≤ A4, 0.1 ≤ A4 ≤ 0.8, and A4 is a set constant.

4. The method for thickening SiC ohmic contact metal after claim 1, characterized in that: The numerical range of the thickness D1 of the metal layer is: greater than or equal to 50 nm and less than or equal to 600 nm. The numerical range of the thickness D2 of the protective layer is: greater than or equal to 10 nm and less than or equal to 2000 nm; The numerical range of the thickness D3 of the remaining protective layer is: greater than 0 and less than or equal to 1000 nm; The numerical range of the thickness D4 of the thickened metal layer is: greater than 50 nm and less than or equal to 6000 nm.

5. The method for thickening SiC ohmic contact metal after claim 4, characterized in that: In step S100, deposit a layer of Ni alloy on the back or front of the SiC wafer, and perform annealing to form a Ni alloy layer with a thickness of D1. The Ni alloy layer with a thickness of D1 is used as the metal layer to complete the ohmic contact fabrication of SiC.

6. The method for thickening SiC ohmic contact metal after claim 5, characterized in that: In step S100, the deposition temperature T1 is 25 degrees - 400 degrees, the annealing time S1 is: 5 min - 15 min, and the deposition method is: evaporation or sputtering.

7. The method for thickening SiC ohmic contact metal after claim 6, characterized in that: In step S200, deposit the protective layer with a thickness of D2 on the metal layer. The deposition temperature T2 is 25 degrees - 400 degrees, and the deposition method is: evaporation or sputtering.

8. The method for thickening SiC ohmic contact metal after claim 7, characterized in that: In the step S200, the protective layer is a metal protective film, and the metal includes Al, Ti, and TiAl alloy.

9. The method for thickening SiC ohmic contact metal after claim 8, characterized in that: In the step S300, at least a portion of the protective layer is wet-etched or dry-etched to form the remaining protective layer with a thickness of D3.

10. The method for thickening SiC ohmic contact metal after claim 9, characterized in that: In the step S400, the thickened metal layer with a thickness of D4 is deposited on the remaining protective layer, the deposition temperature T3 is 25 degrees to 400 degrees, and the deposition method is: evaporation, sputtering, and electroplating.