A low-silicon raw fiber oil for giant tow carbon fiber and its preparation method

By using low-silicon raw silk oils composed of quaternary ammonium salt/alkyl/amino and quaternary ammonium salt/phenyl co-modified silicone oil, the problems of silicon pollution and insufficient mechanical properties in the production of giant tow carbon fibers are solved. The effect of reducing the ash content of carbon fiber and improving the tensile breaking strength is achieved.

CN118326573BActive Publication Date: 2024-10-22JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410568244.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-10-22
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

The existing technology lacks low-silicon raw fiber oil for giant tow carbon fiber with better performance, which leads to problems of silicon contamination and insufficient mechanical properties during the carbon fiber production process.

Method used

It uses quaternary ammonium salt/alkyl/amino co-modified silicone oil and quaternary ammonium salt/phenyl/amino co-modified silicone oil as the main components, combined with heat-resistant organic esters, emulsifiers, antistatic agents and antioxidants to prepare A low-silicon raw fiber oil for giant tow carbon fiber with excellent performance. The oil is in an emulsion state through emulsification treatment.

Benefits of technology

Effectively reduce silicon pollution during the production process of carbon fiber, reduce the ash content of carbon fiber, and improve the tensile breaking strength and mechanical properties of carbon fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004830045710000111
    Figure BDA0004830045710000111
  • Figure BDA0004830045710000121
    Figure BDA0004830045710000121
Patent Text Reader

Abstract

The present invention provides a low-silicon type precursor oil for giant tow carbon fibers and a preparation method thereof, and belongs to the technical field of carbon fiber precursor oil development. The present invention adopts quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil as main components, combined with heat-resistant organic esters, emulsifiers, antistatic agents and antioxidants, to obtain a low-silicon type precursor oil with excellent performance that can be used for giant tow carbon fiber production. The low-silicon type precursor oil for giant tow carbon fibers obtained by the present invention can effectively reduce silicon pollution in the carbon fiber production process, achieve the effect of reducing the ash content of carbon fiber, and can improve the tensile strength and mechanical properties of carbon fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber precursor oil development, and in particular to a low-silicon precursor oil for giant tow carbon fibers and a preparation method thereof. Background Art

[0002] Carbon fiber (CF for short) is an inorganic polymer fiber material. The carbon content in its chemical composition is as high as 90% or more. It has a stable chemical structure and has the characteristics of carbon materials such as electrical conductivity, excellent heat transfer, good chemical stability, good high temperature resistance, good corrosion resistance, and low thermal expansion coefficient. It also has low density, good tensile resistance, and high tensile modulus. Therefore, it can not only be used as a reinforced base load for structural material components, that is, a reinforcing material for high-performance composite materials, but also as a functional material widely used in aerospace rockets and satellites. It is also used in aerospace shuttles, building reinforcement, sports goods, automotive structures, medical equipment and other fields. In recent years, it has been widely used in the reinforcement beams of wind turbine blades, crucible equipment in the photovoltaic industry, etc. Carbon fiber is anisotropic and has good designability, so it can be manufactured into composite material components after calculation. Before use, the carbon fiber is woven into a unidirectional cloth, a fine woven fabric, or a multi-directional cloth, and then combined with a resin matrix to make a certain part. At present, some industries use chopped carbon fiber as a raw material, and then combined with a resin matrix to make carbon felt for application. Compared with other metal structural parts, the composite materials made of carbon fiber through design and other matrices have better mechanical properties, are lighter in weight, and have a longer service life. Therefore, carbon fiber can be called the king of new materials.

[0003] According to the raw materials used to produce carbon fiber, carbon fiber can be divided into three types: polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber, and viscose-based carbon fiber. PAN-based carbon fiber has obvious advantages in terms of strength stability, and asphalt-based carbon fiber is more advantageous in terms of raw material prices; viscose-based carbon fiber is used as ablation-resistant materials in the military field due to its high cost and complex process routes. At present, the leading companies in the world in producing high-performance small-tow carbon fiber are Japan's Toray, Toho and Mitsubishi. At present, it can be defined according to Toray standards, and T300-grade carbon fiber with a median tensile strength of 3500Mpa and a Young's modulus of less than 240Gpa is classified as a general-purpose standard-strength standard-modulus carbon fiber, and carbon fibers with grades above T700 and the M series are called high-performance carbon fibers.

[0004] Another classification method for carbon fiber products is to distinguish them according to the number of single filaments in the bundle. For example, 1,000 or 3,000 single filaments in the bundle are called 1K or 3K. Moreover, 1K, 3K, 6K, 12K, and 24K are also called small-tow carbon fibers. Those greater than 48K are called large-tow carbon fibers, and those greater than or equal to 100K are called giant-tow carbon fibers. At present, the use of carbon fiber in the international industrial market is gradually increasing year by year. Carbon fiber manufacturers have begun to focus on the research and development of engineering production of giant-tow carbon fibers in order to pursue the development direction of reducing costs and increasing market use.

[0005] Oil is one of the main additives in carbon fiber production, and can achieve the following effects in carbon fiber production:

[0006] (1) During the spinning and drying densification process, the oil agent can effectively prevent the adhesion and fusion of the monofilaments. This kind of fusion will lead to uneven oxidation degree, insufficient strength of the oxidized fiber, and burnout during the oxidation stage.

[0007] (2) During the pre-oxidation process, the heat generated by oxidation and cyclization reactions is relatively large. The oil agent can prevent the fibers from sticking together, and the heat can be quickly released and transferred away, effectively preventing thermal winding between the fibers. This winding phenomenon not only causes defects on the fiber surface, but also causes the fiber to burn out, and even causes safety hazards such as combustion.

[0008] (3) During the low-temperature carbonization process of PAN pre-oxidized fibers, the fibers will decompose in the form of tar or gas, about 30% to 40% of their own mass. The highly heat-resistant oil agent will prevent a large amount of tar and other by-products from accumulating on the fiber surface, thereby causing yarn twisting and yarn breakage. Moreover, these by-products will be eliminated simultaneously with the decomposition of the oil agent.

[0009] (4) The oil is evenly coated on the monofilament fiber to form a protective film to prevent the surface wear of the fiber during the production process. Since carbon fiber production is a continuous textile process, the fiber must pass through many transmission and guide rollers during production. Therefore, the oil can play a lubricating role and can effectively reduce the friction between the monofilaments and the friction between the bundle and the equipment during the fiber transmission process.

[0010] Chinese patent CN103601889A discloses a polyol ester modified silicone oil, a preparation method thereof and a carbon fiber oil agent as a key component thereof. A new type of polyol ester modified silicone oil is obtained by directly connecting a polyol ester with good heat resistance to a siloxane side chain, and using it as an essential component of a low-silicon carbon fiber oil agent, thereby fundamentally avoiding the possibility of microscopic phase separation between the polyol ester and the silicone oil, and obtaining an oil agent product with good microscopic compatibility. In addition, since the polyol ester modified silicone oil contains both a siloxane segment on the main chain and a polyol ester segment on the side chain, it has good compatibility with other added silicone oil compounds and organic ester compounds, which is beneficial to reducing costs and adjusting the carbon fiber oil agent formula.

[0011] The prior art still lacks a low-silicon raw fiber oil agent with better performance for giant tow carbon fiber. Summary of the invention

[0012] The purpose of the present invention is to provide a low-silicon raw fiber oil for giant tow carbon fiber to solve the problem of insufficient performance of existing products.

[0013] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0014] The present invention provides a low-silicon type raw fiber oil for giant tow carbon fiber, which is prepared from the following raw materials in parts by weight:

[0015] 6-8 parts of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 2-4 parts of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 4-6 parts of heat-resistant organic ester, 1-5 parts of emulsifier, 1-5 parts of antistatic agent and 0.5-1 part of antioxidant.

[0016] Preferably, the preparation method of the quaternary ammonium salt / alkyl / amino co-modified silicone oil comprises the following steps:

[0017] Octamethylcyclotetrasiloxane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, dodecyl(methyl)dimethoxysilane, dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, hexamethyldisiloxane and an alkali-gel catalyst are mixed and reacted at 110-130° C. for 5-7 hours to obtain an alkyl / amino co-modified silicone oil;

[0018] The alkyl / amino co-modified silicone oil, 2-bromoethyltrimethylammonium bromide and isopropanol are mixed, the temperature is raised to reflux, and the reaction is carried out for 11 to 13 hours to obtain the quaternary ammonium salt / alkyl / amino co-modified silicone oil.

[0019] Preferably, the preparation method of the quaternary ammonium salt / phenyl / amino co-modified silicone oil comprises the following steps:

[0020] Octamethylcyclotetrasiloxane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, diphenyldimethoxysilane, hexamethyldisiloxane and an alkali-gel catalyst are mixed and reacted at 110-130° C. for 5-7 hours to obtain a phenyl / amino co-modified silicone oil;

[0021] Phenyl / amino co-modified silicone oil, 2-bromoethyltrimethylammonium bromide and isopropanol are mixed, the temperature is raised to reflux, and the reaction is carried out for 11 to 13 hours to obtain quaternary ammonium salt / phenyl / amino co-modified silicone oil.

[0022] Preferably, the heat-resistant organic ester is selected from one or more of tetralauryl pyromellitic acid, trilauryl trimellitic acid, trimethylolpropane tristearate, pentaerythritol tetrastearate and dipentaerythritol hexastearate.

[0023] Preferably, the emulsifier is isomeric alcohol polyoxyethylene ether and / or fatty alcohol polyoxyethylene ether.

[0024] Preferably, the antistatic agent is selected from one or more of potassium cetyl sulfate, sorbitan fatty acid ester and polyoxyethylene laurate.

[0025] Preferably, the antioxidant is selected from one or more of 2,6-di-tert-butyl-p-cresol, 2,4-dimethyl-6-tert-butylphenol and dioctadecyl pentaerythritol diphosphite.

[0026] The present invention also provides a method for preparing the above-mentioned low-silicon type precursor oil for giant tow carbon fiber, comprising the following steps:

[0027] The components other than water are mixed and heated, and water is added for emulsification. After emulsification, the mixture is cooled to room temperature, and the pH value of the emulsion is adjusted to neutral to obtain a low-silicon raw fiber oil for giant tow carbon fibers in an emulsion state, which can be used directly.

[0028] Preferably, the heating temperature is 50-70°C.

[0029] Preferably, the emulsification is carried out at a rotation speed of 500 to 2000 r / min;

[0030] The emulsification time is 1 to 3 hours.

[0031] The present invention also provides the low-silicon precursor oil agent for giant tow carbon fibers and the use of the low-silicon precursor oil agent for giant tow carbon fibers obtained by the above-mentioned preparation method in reducing silicon pollution in the carbon fiber production process, reducing the ash content of carbon fibers, and improving the tensile strength and mechanical properties of carbon fibers.

[0032] Beneficial effects of the present invention:

[0033] The present invention adopts quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil as main components, combined with heat-resistant organic ester, emulsifier, antistatic agent and antioxidant, to obtain a low-silicon type precursor oil for giant tow carbon fiber with excellent performance. The low-silicon type precursor oil for giant tow carbon fiber obtained by the present invention can effectively reduce silicon pollution in the carbon fiber production process, achieve the effect of reducing the ash content of carbon fiber, and can improve the tensile strength and mechanical properties of carbon fiber. DETAILED DESCRIPTION

[0034] The present invention provides a low-silicon type raw fiber oil for giant tow carbon fiber, which is prepared from the following raw materials in parts by weight:

[0035] 6-8 parts of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 2-4 parts of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 4-6 parts of heat-resistant organic ester, 1-5 parts of emulsifier, 1-5 parts of antistatic agent and 0.5-1 part of antioxidant.

[0036] In the present invention, the preparation method of the quaternary ammonium salt / alkyl / amino co-modified silicone oil preferably comprises the following steps:

[0037] Octamethylcyclotetrasiloxane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, dodecyl(methyl)dimethoxysilane, dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, hexamethyldisiloxane and an alkali-gel catalyst are mixed and reacted at 110-130° C. for 5-7 hours to obtain an alkyl / amino co-modified silicone oil;

[0038] The alkyl / amino co-modified silicone oil, 2-bromoethyltrimethylammonium bromide and isopropanol are mixed, the temperature is raised to reflux, and the reaction is carried out for 11 to 13 hours to obtain the quaternary ammonium salt / alkyl / amino co-modified silicone oil.

[0039] The preparation method of the quaternary ammonium salt / alkyl / amino co-modified silicone oil is further preferably:

[0040] 296.62g of octamethylcyclotetrasiloxane, 61.91g of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, 82.35g of dodecyl(methyl)dimethoxysilane, 60.68g of dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, 16.24g of hexamethyldisiloxane and 1.82g of alkali gel catalyst were heated to 120°C under nitrogen protection, stirred for reaction for 6h, and low boiling points were removed under reduced pressure to obtain alkyl / amino co-modified silicone oil.

[0041] 220.06g of alkyl / amino co-modified silicone oil, 12.35g of 2-bromoethyltrimethylammonium bromide and 200mL of isopropanol were added into a 500mL three-necked flask with a mechanical stirrer and a condenser. The temperature was raised to reflux under nitrogen protection and the reaction was stirred for 12h. After the reaction was completed, the solvent and low-boiling substances were removed under reduced pressure to obtain a light yellow viscous quaternary ammonium salt / alkyl / amino co-modified silicone oil.

[0042] In the present invention, the preparation method of the quaternary ammonium salt / phenyl / amino co-modified silicone oil preferably comprises the following steps:

[0043] Octamethylcyclotetrasiloxane, hexamethyldisiloxane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, diphenyldimethoxysilane and an alkali-gel catalyst are mixed and reacted at 110-130° C. for 5-7 hours to obtain a phenyl / amino co-modified silicone oil;

[0044] Phenyl / amino co-modified silicone oil, 2-bromoethyltrimethylammonium bromide and isopropanol are mixed, the temperature is raised to reflux, and the reaction is carried out for 11 to 13 hours to obtain quaternary ammonium salt / phenyl / amino co-modified silicone oil.

[0045] The preparation method of the quaternary ammonium salt / phenyl / amino co-modified silicone oil is further preferably:

[0046] 296.62g of octamethylcyclotetrasiloxane, 8.12g of hexamethyldisiloxane, 61.91g of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, 73.38g of diphenyldimethoxysilane, and 1.82g of alkali rubber catalyst were added into a 500mL three-necked flask, heated to 120°C under nitrogen protection, stirred for reaction for 6h, and then reduced pressure to remove low boiling points to obtain phenyl / amino co-modified silicone oil.

[0047] 224.19 g of phenyl / amino co-modified silicone oil, 12.35 g of 2-bromoethyltrimethylammonium bromide, and 200 mL of isopropanol were added to a 500 mL three-necked flask with a mechanical stirrer and a condenser. The temperature was raised to reflux under nitrogen protection, and the reaction was stirred for 12 hours. After the reaction was completed, the solvent and low-boiling substances were removed under reduced pressure to obtain a light yellow viscous quaternary ammonium salt / phenyl / amino co-modified silicone oil.

[0048] In the present invention, the heat-resistant organic ester is selected from one or more of tetralauryl pyromellitic acid, trilauryl trimellitic acid, trimethylolpropane tristearate, pentaerythritol tetrastearate, and dipentaerythritol hexastearate; the emulsifier is preferably isomeric alcohol polyoxyethylene ether and / or fatty alcohol polyoxyethylene ether (AEO-3, AEO-5 or AEO-9, etc.); the antistatic agent is preferably selected from one or more of potassium hexadecanol sulfate, sorbitan fatty acid ester and polyoxyethylene laurate; the antioxidant is preferably selected from 2,6- One or more of di-tert-butyl-p-cresol, 2,4-dimethyl-6-tert-butylphenol and dioctadecyl pentaerythritol diphosphite; the raw materials of the low-silicon raw fiber oil for giant tow carbon fiber described in the present invention also preferably include other additives, such as defoaming agents or pH regulators, wherein the defoaming agent can defoam the carbon fiber oil emulsion to avoid the presence of foam in the carbon fiber oil emulsion and the adverse effects on the subsequent production process and product quality; the pH regulator can adjust the pH value of the carbon fiber oil, and the additives can be conventional products in the field.

[0049] The present invention also provides a method for preparing the above-mentioned low-silicon type precursor oil for giant tow carbon fiber, comprising the following steps:

[0050] The other components except water are mixed and heated, and water is added for emulsification. After the emulsification is completed, the mixture is cooled to room temperature, and the pH value of the emulsion is adjusted to neutral to obtain a low-silicon type raw fiber oil for giant tow carbon fiber in an emulsion state, which can be directly used; the heating temperature is preferably 50-70°C; the emulsification is preferably carried out at a rotation speed of 500-2000r / min; and the emulsification time is preferably 1-3h.

[0051] The present invention also provides the low-silicon precursor oil agent for giant tow carbon fibers and the use of the low-silicon precursor oil agent for giant tow carbon fibers obtained by the above-mentioned preparation method in reducing silicon pollution in the carbon fiber production process, reducing the ash content of carbon fibers, and improving the tensile strength and mechanical properties of carbon fibers.

[0052] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0053] Example 1

[0054] Preparation method of quaternary ammonium salt / alkyl / amino co-modified silicone oil:

[0055] 296.62g of octamethylcyclotetrasiloxane, 61.91g of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, 82.35g of dodecyl(methyl)dimethoxysilane, 60.68g of dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, 16.24g of hexamethyldisiloxane and 1.82g of alkali gel catalyst were heated to 120°C under nitrogen protection, stirred for reaction for 6h, and low boiling points were removed under reduced pressure to obtain alkyl / amino co-modified silicone oil with a yield of 85%.

[0056] 260.58g of alkyl / amino co-modified silicone oil, 12.35g of 2-bromoethyltrimethylammonium bromide and 200mL of isopropanol were added into a 500mL three-necked flask with a mechanical stirrer and a condenser. The temperature was raised to reflux under nitrogen protection and the reaction was stirred for 12h. After the reaction was completed, the solvent and low-boiling substances were removed under reduced pressure to obtain a light yellow viscous quaternary ammonium salt / alkyl / amino co-modified silicone oil with a yield of 95%.

[0057] Preparation method of quaternary ammonium salt / phenyl / amino co-modified silicone oil:

[0058] 296.62g of octamethylcyclotetrasiloxane, 8.12g of hexamethyldisiloxane, 61.91g of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, 73.38g of diphenyldimethoxysilane, and 1.82g of alkali rubber catalyst were added into a 500mL three-necked flask, heated to 120°C under nitrogen protection, stirred for reaction for 6h, and then low-boiling substances were removed under reduced pressure to obtain phenyl / amino co-modified silicone oil with a yield of 85%.

[0059] 181.01 g of phenyl / amino co-modified silicone oil, 13.25 g of 2-bromoethyltrimethylammonium bromide, and 200 mL of isopropanol were added to a 500 mL three-necked flask with a mechanical stirrer and a condenser. The temperature was raised to reflux under nitrogen protection, and the reaction was stirred for 12 h. After the reaction was completed, the solvent and low-boiling substances were removed under reduced pressure to obtain a light yellow viscous quaternary ammonium salt / phenyl / amino co-modified silicone oil with a yield of 90%.

[0060] Preparation of oil:

[0061] 70g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 30g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of tetralauryl pyromellitic acid, 550g of fatty alcohol polyoxyethylene ether AEO-5, 40g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0062] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0063] Example 2

[0064] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0065] Preparation of oil:

[0066] 60g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 30g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of trimesic acid trilaurate, 50g of fatty alcohol polyoxyethylene ether AEO-9, 40g of polyoxyethylene laurate and 5g of 2,6-di-tert-butyl-p-cresol;

[0067] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0068] Example 3

[0069] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0070] Preparation of oil:

[0071] 80g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 20g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of trimethylolpropane tristearate, 550g of fatty alcohol polyoxyethylene ether AEO-5, 40g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0072] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0073] Example 4

[0074] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0075] Preparation of oil:

[0076] 60g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 40g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of pentaerythritol tetrastearate, 550g of fatty alcohol polyoxyethylene ether AEO-5, 40g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0077] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0078] Example 5

[0079] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0080] Preparation of oil:

[0081] 70g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 30g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of dipentaerythritol hexastearate, 20g of fatty alcohol polyoxyethylene ether AEO-5, 30g of sorbitan fatty acid ester and 10g of 2,6-di-tert-butyl-p-cresol;

[0082] The above raw materials were mixed, heated to 70°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0083] Example 6

[0084] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0085] Preparation of oil:

[0086] 70g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 30g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of trimethylolpropane tristearate, 40g of fatty alcohol polyoxyethylene ether AEO-3, 20g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0087] The above raw materials were mixed, heated to 50°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0088] Comparative Example 1

[0089] The preparation method of quaternary ammonium salt / alkyl / amino co-modified silicone oil is the same as that in Example 1.

[0090] Preparation of oil:

[0091] 100g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 50g of tetralauryl pyromellitic acid, 550g of fatty alcohol polyoxyethylene ether AEO-5, 40g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0092] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0093] Comparative Example 2

[0094] The preparation method of quaternary ammonium salt / phenyl / amino co-modified silicone oil is the same as that in Example 1.

[0095] Preparation of oil:

[0096] 100g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of tetralauryl pyromellitic acid, 550g of fatty alcohol polyoxyethylene ether AEO-5, 40g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0097] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0098] Comparative Example 3

[0099] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0100] Preparation of oil:

[0101] 20g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 80g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of tetralauryl pyromellitic acid, 550g of fatty alcohol polyoxyethylene ether AEO-5, 40g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0102] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0103] Comparative Example 4

[0104] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0105] Preparation of oil:

[0106] 50g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 50g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of tetralauryl pyromellitic acid, 550g of fatty alcohol polyoxyethylene ether AEO-5, 40g of sorbitan fatty acid ester and 5g of 2,6-di-tert-butyl-p-cresol;

[0107] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0108] Comparative Example 5

[0109] The preparation methods of quaternary ammonium salt / alkyl / amino co-modified silicone oil and quaternary ammonium salt / phenyl / amino co-modified silicone oil are the same as those in Example 1.

[0110] Preparation of oil:

[0111] 70g of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 30g of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 50g of tetralauryl pyromellitic acid, 50g of fatty alcohol polyoxyethylene ether AEO-5, 40g of dodecyl hydroxypropyl dihydroxyethyl methyl ammonium sulfate and 5g of 2,6-di-tert-butyl-p-cresol;

[0112] The above raw materials were mixed, heated to 60°C, 3 kg of water was slowly added at a speed of 1000 r / min, and the speed was maintained for 2 hours. After emulsification, it was cooled to room temperature, and the pH value of the emulsion was adjusted to neutral to obtain a low-silicon raw fiber oil agent for giant tow carbon fiber in an emulsion state.

[0113] Experimental example

[0114] The giant tow carbon fiber obtained in Examples 1 to 3 and Comparative Examples 1 to 5 was used as a sample with a low-silicon type raw fiber oil, and the following tests were performed:

[0115] Stability test: Use a centrifuge to centrifuge the oil emulsion at 3000r / min for 30min, and it is considered centrifugal stable if no stratification occurs; leave the oil emulsion at room temperature for 12 months, and it is considered storage stable if no stratification occurs; freeze the oil emulsion in a refrigerator for 5 days, take it out and thaw it at room temperature for 1 day, and it is considered ice-thaw stable if no stratification occurs; if the oil emulsion meets the requirements of centrifugal stability, storage stability and ice-thaw stability at the same time, it is considered stable.

[0116] Production performance test:

[0117] The oil emulsion was diluted with deionized water to a 2.0wt% emulsion, and used to oil the raw fibers in the production of giant tow carbon fibers to produce carbon fibers, wherein each group of raw materials and production processes remained consistent, and the oil adhesion amount, specific resistivity, ash content, tensile breaking strength and elongation at break of the obtained carbon fibers were measured.

[0118] The results are shown in Table 1 below:

[0119] Table 1 Test results of each sample

[0120]

[0121]

[0122] It can be seen from the test results that the carbon fiber oil agent provided by the present invention has optimal performance and can be used to reduce silicon pollution in the carbon fiber production process, reduce the ash content of carbon fiber, and improve the tensile strength and mechanical properties of carbon fiber.

[0123] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A low-silicon raw fiber oil for giant tow carbon fiber, characterized in that: Prepared from the following raw materials in parts by weight: 6-8 parts of quaternary ammonium salt / alkyl / amino co-modified silicone oil, 2-4 parts of quaternary ammonium salt / phenyl / amino co-modified silicone oil, 4-6 parts of heat-resistant organic ester, 1-5 parts of emulsifier, 1-5 parts of antistatic agent and 0.5-1 part of antioxidant; The preparation method of the quaternary ammonium salt / alkyl / amino co-modified silicone oil comprises the following steps: Octamethylcyclotetrasiloxane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, dodecyl(methyl)dimethoxysilane, dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, hexamethyldisiloxane and an alkali-gel catalyst are mixed and reacted at 110-130° C. for 5-7 hours to obtain an alkyl / amino co-modified silicone oil; Mixing alkyl / amino co-modified silicone oil, 2-bromoethyltrimethylammonium bromide and isopropanol, heating to reflux, and reacting for 11 to 13 hours to obtain quaternary ammonium salt / alkyl / amino co-modified silicone oil; The preparation method of the quaternary ammonium salt / phenyl / amino co-modified silicone oil comprises the following steps: Octamethylcyclotetrasiloxane, hexamethyldisiloxane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, diphenyldimethoxysilane and an alkali-gel catalyst are mixed and reacted at 110-130° C. for 5-7 hours to obtain a phenyl / amino co-modified silicone oil; Phenyl / amino co-modified silicone oil, 2-bromoethyltrimethylammonium bromide and isopropanol are mixed, the temperature is raised to reflux, and the reaction is carried out for 11 to 13 hours to obtain quaternary ammonium salt / phenyl / amino co-modified silicone oil.

2. The low-silicon type raw fiber oil for giant tow carbon fiber according to claim 1, characterized in that: The heat-resistant organic ester is selected from one or more of tetralauryl pyromellitic acid, trilauryl trimellitic acid, trimethylolpropane tristearate, pentaerythritol tetrastearate and dipentaerythritol hexastearate.

3. The low-silicon type raw fiber oil for giant tow carbon fiber according to claim 1, characterized in that: The emulsifier is isomeric alcohol polyoxyethylene ether and / or fatty alcohol polyoxyethylene ether.

4. The low-silicon type raw fiber oil for giant tow carbon fiber according to claim 1, characterized in that: The antistatic agent is selected from one or more of potassium hexadecanol sulfate, sorbitan fatty acid ester and polyoxyethylene laurate.

5. The low-silicon type raw fiber oil for giant tow carbon fiber according to claim 1, characterized in that: The antioxidant is selected from one or more of 2,6-di-tert-butyl-p-cresol, 2,4-dimethyl-6-tert-butylphenol and dioctadecyl pentaerythritol diphosphite.

6. The method for preparing the low-silicon type raw fiber oil for giant tow carbon fiber according to any one of claims 1 to 4, characterized in that: The following steps are involved: The components other than water are mixed and heated, and water is added for emulsification. After emulsification, the mixture is cooled to room temperature, and the pH value of the emulsion is adjusted to neutral to obtain a low-silicon raw fiber oil for giant tow carbon fibers in an emulsion state, which can be used directly.

7. The method for preparing a low-silicon raw fiber oil for giant tow carbon fiber according to claim 6, characterized in that: The heating temperature is 50-70°C; the emulsification is carried out at a speed of 500-2000 r / min; The emulsification time is 1 to 3 hours.

8. Use of the low-silicon precursor oil for giant tow carbon fibers as described in any one of claims 1 to 4 and the low-silicon precursor oil for giant tow carbon fibers obtained by the preparation method described in claim 6 in reducing silicon pollution in the carbon fiber production process, reducing the ash content of carbon fibers, and improving the tensile strength and mechanical properties of carbon fibers.