A water-plastic polymer material based on ionic bond / hydrogen bond interaction, preparation method, recycling method and application thereof

By combining the polymerization of nanocellulose fibers with quaternary ammonium acrylate monomers and other materials based on ionic bond/hydrogen bond interaction, the problem of insufficient mechanical properties and shape stability of water plastic polymers is solved. It achieves high mechanical properties and recyclability, solves the problem of non-degradable polymer recycling, and meets the requirements of sustainable development.

CN118344541BActive Publication Date: 2024-11-05NANJING FORESTRY UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410608865.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-11-05
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

The existing water-plastic polymers have poor mechanical properties and insufficient shape stability, which limits their practical application potential, and the problem of recycling and reuse of non-degradable polymers has not been effectively solved.

Method used

Using an ionic/hydrogen bond interaction based water-plastic polymer material prepared by polymerization of nanocellulose fibers with quaternary ammonium acrylate monomers, acrylate-based monomers and polyethylene glycol acrylate monomers, and by wet deformation The method achieves shape stability and is reused physically or chemically, with excellent mechanical properties and geometric stability.

Benefits of technology

It has achieved the improvement of the mechanical properties of water-plastic polymers, extended shape stability, and can be recycled and reused to avoid environmental pollution of non-degradable waste, meets the requirements of sustainable development, has broad industrial prospects and maximizes resource utilization .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118344541B_ABST
    Figure CN118344541B_ABST
Patent Text Reader

Abstract

The present invention discloses a water-plastic polymer material based on ionic bond / hydrogen bond interaction, a preparation method, a recycling method and an application thereof. The water-plastic polymer material based on ionic bond / hydrogen bond interaction has a general structural formula: #imgabs0# wherein a, b and c are positive integers, and 1≤a≤1000, 1≤b≤1000, 1≤c≤1000; a:b:c=(1‑10):(10‑1):(10‑1). R 1 Is: ‑COOH or ‑CH 2 Any one of COOH; R 2 Is: ‑H or ‑CH 3 Any one of R 3 Is: ‑H or ‑CH 3 Any one of R 4 Any one of #imgabs1##imgabs2#; R 5 Is: ‑H or ‑CH 3 Any one of R 6 Is: ‑H or ‑CH 2 Any one of CH. The water-plastic polymer material of the present invention exhibits excellent mechanical properties, can be easily transformed into various stable shapes by a simple wet deformation method, and shows excellent geometric stability at 90% relative humidity for more than 9 months; and can be deconstructed by physical or chemical recycling methods, and has good recycling performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a water-plastic polymer material based on ionic bond / hydrogen bond interaction, a preparation method, a recycling method and application thereof, and belongs to the technical field of self-repairing materials. Background Art

[0002] Non-degradable polymers widely used in transportation, construction, transportation and wind turbine blades are difficult to recycle, resulting in the continuous accumulation of non-degradable waste, causing serious environmental pollution and economic problems. The reuse of non-degradable polymers is a difficult task.

[0003] In recent years, the research on the recycling, reshaping and reuse of polymers using water has attracted much attention. The development of water-plastic polymers is expected to alleviate the problem of the difficulty in recycling and reusing non-degradable waste. However, the active dynamic network structure of water-plastic polymers leads to poor mechanical properties and the inability to maintain a stable shape for a long time, which limits their practical application potential. Summary of the invention

[0004] In order to solve the problems of poor mechanical properties and insufficient shape stability of water-plastic polymers in the prior art, the present invention provides a water-plastic polymer material based on ionic bond / hydrogen bond interaction, a preparation method, a recycling method and applications thereof.

[0005] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:

[0006] A water-plastic polymer material based on ionic bond / hydrogen bond interaction, the general structural formula of which is:

[0007]

[0008] Wherein, a, b and c are positive integers, and 1≤a≤1000, 1≤b≤1000, 1≤c≤1000; a:b:c=(1-10):(10-1):

[0009] (10-1). R1 ​​is: -COOH or -CH2COOH;

[0010] R2 is: any one of -H or -CH3;

[0011] R3 is: any one of -H or -CH3;

[0012] R4 is: Any of the following;

[0013] R5 is: any one of -H or -CH3;

[0014] R6 is any one of -H or -CH2CH.

[0015] The above-mentioned water-plastic polymer material exhibits excellent mechanical properties and fully meets the needs of daily use; thanks to the dynamic bonding of ionic bonds and hydrogen bonds in the structure, it is easy to transform into various stable shapes through a simple wet deformation method, and shows excellent geometric stability at 90% relative humidity for more than 9 months. In addition, the material can be deconstructed through physical or chemical recycling methods, has good recycling performance, and meets the requirements of sustainable development.

[0016] The water-plastic polymer material has excellent water resistance and stability at room temperature. The water-plastic polymer material is softened and plasticized after being soaked in hot water at 50-60°C for 25-30 minutes.

[0017] The water-plastic polymer material based on ionic bond / hydrogen bond interaction is prepared by polymerizing nanocellulose fibers with quaternary ammonium salt acrylate monomers, acrylic acid-based monomers and polyethylene glycol acrylate monomers.

[0018] As one specific implementation scheme, the method for preparing the water-plastic polymer material based on ionic bond / hydrogen bond interaction comprises the following steps:

[0019] a. Using bleached conifer pulp as raw material, preparing a nanocellulose fiber dispersion by catalytic oxidation with 2,2,6,6-tetramethylpiperidinyl oxide;

[0020] b. The nanocellulose fiber dispersion obtained in step a is uniformly mixed with quaternary ammonium salt acrylate monomer, acrylic acid-based monomer and polyethylene glycol acrylate monomer, and a water-plastic polymer material is prepared by ultraviolet light curing polymerization.

[0021] In order to improve the yield, as one of the preferred implementation schemes, step a is: sodium bromide, 2,2,6,6-tetramethylpiperidine-1-oxyl free radical, deionized water and bleached conifer pulp are mixed at room temperature, sodium hypochlorite solution (effective chlorine mass content is 13-16%), and the pH is adjusted to within the range of 10-10.2 with an alkaline solution. The reaction is carried out until the pH is stable (about 6 to 10 hours), and the reaction is considered to have reached the oxidation endpoint; solvent 1 is used to wash until the filtrate pH is neutral and the ion conductivity is less than 50 μS / cm, the slurry is collected and treated with a homogenizer to obtain a nanocellulose fiber dispersion, which is stored in a refrigerator at 4°C.

[0022] The sodium hypochlorite solution is added in a slow dripping manner, with a slow dripping speed of 2 to 3 seconds per drop. The alkaline solution for pH adjustment is preferably a NaOH solution with a concentration of 1 mol / L.

[0023] In order to improve the reaction efficiency, in step a, the mass ratio of sodium bromide to 2,2,6,6-tetramethylpiperidin-1-oxyl free radical is (8-10):(0.8-10); the ratio of the mass g of bleached conifer pulp to the volume mL of sodium hypochlorite solution is (0.5-1):(2.5-3.5).

[0024] In order to ensure product quality, in step a, solvent 1 is at least one of deionized water or ethanol.

[0025] In order to improve the yield, as one of the preferred implementation schemes, step b is: the nanocellulose fiber dispersion obtained in step a is evenly mixed with quaternary ammonium salt acrylate monomer, acrylic acid-based monomer and polyethylene glycol acrylate monomer, and a water-plastic polymer material is prepared by ultraviolet light curing polymerization.

[0026] In order to improve the yield and take into account the product performance, as one of the preferred implementation schemes, step b is: dissolving the quaternary ammonium salt acrylate monomer, the acrylic acid monomer and the polyethylene glycol acrylate monomer in the nanocellulose dispersion, stirring for 10 to 20 minutes, adding 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone and mixing evenly, performing three cryopump thawing cycles and degassing treatment, and then pouring the obtained monomer mixture into a polytetrafluoroethylene mold, and polymerizing by ultraviolet irradiation for 1 to 2 hours (365nm exposure, average intensity of 30mW cm -2 ) to obtain a water-plastic polymer material based on ionic bond / hydrogen bond interaction.

[0027] In order to take into account both reaction efficiency and product performance, in step b, the acrylic acid-based monomer is at least one of acrylic acid and methacrylic acid; the polyethylene glycol acrylate monomer is at least one of methacrylate polyethylene glycol methacrylate, polyethylene glycol acrylate monomethyl ether or polyethylene glycol diacrylate; the quaternary ammonium salt acrylate monomer is at least one of acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, N-(2-acryloyloxyethyl)-N-benzyl-N,N-dimethylammonium chloride or 3-[[2-(methacryloyloxy)ethyl]dimethylammonium] propionate; the mass ratio of the quaternary ammonium salt acrylate monomer, the acrylic acid-based monomer, the polyethylene glycol acrylate monomer and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone is (0.30-1.55):(4.0-15.5):(4.0-15.5):(0.01-0.20).

[0028] In order to enhance product performance, in step b, the mass ratio of the total mass of the quaternary ammonium salt acrylate monomer, the acrylic acid monomer and the polyethylene glycol acrylate monomer to the nanocellulose dispersion is (0.5-5.0):(10-50); the nanocellulose dispersion obtained in step a is a carboxylated nanocellulose dispersion; and the solid content of the nanocellulose dispersion is 1-2%.

[0029] The above-mentioned water-plastic polymer material based on ionic bond / hydrogen bond interaction can be recycled, and the recycling has little effect on the product performance. The above-mentioned water-plastic polymer material based on ionic bond / hydrogen bond interaction can be recycled by physical or chemical methods. Preferably, the recycling method is: cut the material into pieces of 0.1-5 mm 2 (surface area), flatten, and hot press at a temperature of 35-40°C and a pressure of 2-3 MPa for 0.5-1 h. Alternatively, cut the material into pieces of 0.1-1 mm 2 , immersed in water, add ammonium carbonate aqueous solution, react at 70-80°C for 1-2 hours, pour into a polytetrafluoroethylene mold and dry and solidify (dry at 50-60°C for 8-10 hours); wherein the mass ratio of waste materials, water and ammonium carbonate aqueous solution is: (0.1-5.0): (10-50): (1-10).

[0030] The tensile strength of the water-plastic polymer material based on ionic / hydrogen bond interactions is significantly higher than that of current commercial plastics, and can replace existing plastics. At the same time, the water-plastic polymer material based on ionic / hydrogen bond interactions in the present application also has excellent self-healing properties and material stability, and can be recycled.

[0031] The technologies not mentioned in the present invention are all referred to the prior art.

[0032] The beneficial effects of the present invention are:

[0033] 1. The production process of the present invention is short, the raw materials are easily available, the reaction conditions are mild, and it has broad industrial prospects.

[0034] 2. The recycling and reuse of non-degradable waste has aroused the consideration of environmental pollution and sustainable economy. The present invention uses nanocellulose as raw material to construct a water-plastic polymer with high mechanical properties, recyclability, remodelability and self-healing, which has great development potential.

[0035] 3. The present invention prepares a high-strength and high-stability water-plastic polymer material by constructing a dynamic network structure driven by water molecules. It can be easily transformed into various stable shapes through a simple wet deformation method and shows excellent geometric stability at 90% relative humidity for more than 9 months.

[0036] 4. The water-plastic polymer material prepared by the present invention can be recycled through physical or chemical means, has excellent recycling performance, avoids environmental problems caused by waste, achieves maximum resource utilization, and meets the requirements of sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a transmission electron microscopy image of the nanocellulose fibers prepared in Example 1.

[0038] Figure 2 This is the infrared spectrum of the nanocellulose fibers prepared in Example 1.

[0039] Figure 3 This is the solid state carbon nuclear magnetic resonance spectrum of the nanocellulose fibers prepared in Example 1.

[0040] Figure 4 This is a flow chart for preparing the water-plastic polymer material of Example 1.

[0041] Figure 5 This is a physical picture of the water-plastic polymer material prepared in Example 1.

[0042] Figure 6 This is a schematic diagram of the structure of the water-plastic polymer material prepared in Example 1.

[0043] Figure 7 This is the infrared spectrum of the water-plastic polymer material prepared in Example 1.

[0044] Figure 8 The scanning electron microscope image and energy dispersive X-ray spectrometer spectrum of the water-plastic polymer material prepared in Example 1 are shown.

[0045] Fig. 9 This is the dynamic thermomechanical analysis spectrum of the water-plastic polymer material prepared in Example 1.

[0046] Fig.10 This is a comparison chart of the mechanical properties of the water-plastic polymer material prepared in Example 1 in a stable state and a water-plastic state.

[0047] Fig.11 This is a comparison chart of the tensile strength of the water-plastic polymer material prepared in Example 1 and commercial plastics.

[0048] Fig.12 The plasticity diagram of the water-plastic polymer material prepared in Example 1 and its shape stability performance in a high humidity environment.

[0049] Fig.13 This is a self-healing diagram of the water-plastic polymer material prepared in Example 1.

[0050] Fig.14Schematic diagram of two different recycling methods for the water-plastic polymer material prepared in Example 1.

[0051] Fig.15 This is a comparison chart of the tensile strength of the water-plastic polymer material prepared in Example 1 before and after recycling. DETAILED DESCRIPTION

[0052] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0053] Unless otherwise specified in the examples, the reaction was carried out at room temperature (15 to 25° C.).

[0054] Example 1

[0055] Take 15g of bleached conifer pulp (Shijiazhuang Tengbang Mineral Products Co., Ltd.) and add it to 1000mL of deionized water and disperse it evenly by stirring. Add 1.5g of sodium bromide and 0.25g of 2,6,6-tetramethylpiperidin-1-oxyl free radical and stir it evenly at room temperature; then use a constant pressure funnel to drip 40mL of sodium hypochlorite solution (effective chlorine mass content is 15wt%) into the above system at a rate of 30 drops / min, and use 0.1M NaOH solution to adjust the pH of the system to the range of 10-10.2. The reaction is carried out for 8 hours (including the dripping time of sodium hypochlorite solution). The pH remains stable and the reaction reaches the oxidation endpoint; use deionized water to wash until the filtrate pH is neutral and the ion conductivity is less than 50μS / cm, collect the pulp and treat it with a homogenizer to obtain a nanocellulose fiber dispersion (CNF), which is stored in a refrigerator at 4°C for use. Figure 1 As shown in Figure 2, the transmission electron microscopy image of the nanocellulose fibers verifies the morphology of the nanocellulose fibers and shows the typical nanofiber morphology. Figure 2 As shown: Nanocellulose fibers obtained after 2,2,6,6-tetramethylpiperidin-1-oxyl free radical oxidation at 1604 cm -1 The absorption peak near is attributed to the asymmetric stretching of -COO-. The solid-state NMR carbon spectrum of nanocellulose fibers is shown in Figure 3 As shown, it is proved that the characteristic chemical shifts of cellulose are at 65.37ppm (C-6), 71.65ppm, 74.31ppm, 75.07ppm (C-2, C-3 and C-5), 88.96ppm (C-4) and 104.76ppm (C-1). In addition, obvious chemical shifts are observed at 173.25ppm (C-7, -COOH).

[0056] like Figure 4As shown, 1 g of acryloyloxyethyl trimethylammonium chloride (purchased from McLean), 5 g of acrylic acid and 4.5 g of polyethylene glycol acrylate monomethyl ether (purchased from Aladdin, average molecular weight 2000) were dissolved in 20 g of nanocellulose dispersion (solid content 1.5%), stirred for 20 min, 0.1 g of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (purchased from McLean) was added and mixed evenly, and three liquid nitrogen cooling-vacuuming-thawing cycles were performed, and then the obtained material was quickly (the operation was completed within 1 minute) poured into a polytetrafluoroethylene mold, and polymerized by ultraviolet irradiation for 2 hours (365 nm exposure, average intensity 30 mW cm -2 ), a transparent and soft water-plastic polymer material (Cel-PGAD) was prepared based on ionic / hydrogen bonding interactions ( Figure 5 ), whose structure is as follows Figure 6 shown.

[0057] Effect evaluation:

[0058] Figure 7 The infrared spectrum of water-plastic polymer material (Cel-PGAD) is shown. Figure 7 As shown, 1637cm -1 The double bond at 1480cm disappeared after the polymerization reaction, indicating that the polymerization of the water plastic material (Cel-PGAD) was completed. -1 The characteristic peaks near belong to (CH3)3N + , 1690cm -1 The absorption band at is attributed to the stretching vibration peak of the carboxylate (COO-) group of MAA in the copolymer system. In Cel-PGAD, almost all charged groups exist in the form of ionic bonds, v(COO-) moves to a higher wave number, and v(CN) moves to a lower wave number, which indicates that the self-associated [N(CH3)3] + :[COO-] ion pair generation. Scanning electron microscope image ( Figure 8 ) shows that the surface of the water-plastic polymer material is smooth and flat, and the energy dispersive X-ray spectrometer spectrum also shows the uniform distribution of C, O, N, and Cl. Dynamic thermomechanical analysis spectrum ( Fig. 9 ) shows the glass transition temperature (T g ) is 15.8℃.

[0059] The tensile strength of water-plastic polymer materials is Fig.10 and Fig.11As shown in the figure, the tensile strength of the material in the stable state (Rigid state, after being prepared, stored under ambient conditions for 24 hours) reached 77.53MPa, which is 16.1 times higher than the tensile strength in the soft state (in 50°C hot water). At the same time, the Young's modulus and toughness of the water-plastic polymer material reached 1.88GPa and 29.03MJ / m 3 , which are 8.2 and 7.5 times stronger than those in the water plastic state. Fig.11 As shown in the figure, the tensile strength of the water-plastic polymer material is much higher than the tensile strength of the currently commercially used low-density polyethylene (LDPE), high-density polyethylene (HDPE), polypropylene (PP), polystyrene (PS), acrylonitrile-butadiene-styrene polymer (ABS), soft polyvinyl chloride (soft PVC) and degradable plastics [polybutylene adipate-terephthalate co-ester (PBAT), polyhydroxyalkanoate (PHA), polyhydroxybutyrate-valerate (PHBV), polybutylene succinate (PBS), polycaprolactone (PCL), polylactic acid (PLA) and other plastics]. This material has broad application prospects as a substitute for non-degradable plastics.

[0060] like Fig.12 As shown in the figure, the shape stability of the water-plastic polymer material under different humidity environments was evaluated. The water-plastic polymer material showed excellent shape stability at 30% RH, 60% RH and 90% RH, and no damage or deformation occurred after 9 months (room temperature). The self-healing property of the water-plastic polymer material is shown in the figure. Fig.13 As shown, based on the abundant ionic bonds / hydrogen bonds in the dynamic network structure, it exhibits excellent self-healing properties. Scratches were made on the surface of the material to produce damage, and the healing process was monitored using an optical microscope. The damaged water-plastic polymer material (scar width of 35μm and depth of 50μm) was placed at 25°C, 60% RH for 5 minutes. The damage of the material was significantly improved and the cracks became significantly shallower. By extending the placement time, the cracks were almost completely healed after 10 minutes, and completely healed after 20 minutes. The self-healing efficiency was as high as over 90%. In addition, the water-plastic polymer material exhibits excellent recyclability. As Fig.14 and Fig.15 As shown, the water-plastic polymer material can be recycled by physical methods (recycling route I, specific implementation method: cut the waste material into pieces of 0.1-3 mm 2 , flattened, hot pressed for 1 h at 40 ° C and 3 MPa using a flat hot press) and chemical method (recycling route II, specific implementation method: 1g of waste material is cut into pieces of 0.1-1mm 2, immersed in 20g of water, added with 5g of 1M ammonium carbonate aqueous solution, stirred and dissolved at 80°C for 2h, poured into a polytetrafluoroethylene mold and dried and cured at 50°C for 10h) for recycling and reuse. Even after multiple recycling and reprocessing, the tensile strength of the water-plastic polymer material still reached above 70MPa.

[0061] The water-plastic polymer material becomes soft and plastic after being soaked in hot water at 50°C for 30 minutes.

[0062] Example 2

[0063] 15 g of bleached conifer pulp (Shijiazhuang Tengbang Mineral Products Co., Ltd.) was added to 1000 mL of deionized water and dispersed evenly by stirring, and 1.8 g of sodium bromide and 0.2 g of 2,6,6-tetramethylpiperidin-1-oxyl free radical were added and stirred evenly at room temperature; then 40 mL of sodium hypochlorite solution (with an effective chlorine content of 15 wt%) was dripped into the above system at a rate of 30 drops / min using a constant pressure funnel, and the pH of the system was adjusted to within the range of 10-10.2 using a 0.1 M NaOH solution, and the reaction was carried out for 10 hours (including the dripping time of the sodium hypochlorite solution), the pH remained stable, and the reaction reached the oxidation endpoint; deionized water was used to wash until the filtrate pH was neutral and the ionic conductivity was less than 50 μS / cm, the slurry was collected and treated with a homogenizer to obtain a nanocellulose fiber dispersion, which was stored in a refrigerator at 4°C for use.

[0064] 2g of acryloyloxyethyl trimethylammonium chloride (purchased from McLean), 4g of methacrylic acid and 4.5g of polyethylene glycol diacrylate (purchased from Aladdin, average molecular weight 1000) were dissolved in 25g of nanocellulose dispersion (solid content 1.5%), stirred for 20min, 0.12g of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (purchased from McLean) was added and mixed evenly, and three liquid nitrogen cooling-vacuuming-thawing cycles were performed. Then the obtained material was quickly (the operation was completed within 1 minute) poured into a polytetrafluoroethylene mold. The polymerization was carried out under ultraviolet irradiation for 1 hour (365nm exposure, average intensity 30mW cm -2 ) prepared water-plastic polymer materials based on ionic bond / hydrogen bond interactions.

[0065] The tensile strength of the water-plastic polymer material prepared above reaches 75.3MPa; it shows excellent water-plastic molding and long-term shape stability performance, and the shape stability at room temperature and 90% RH is greater than 9 months. The water-plastic polymer material can almost completely repair scratches with a width of 30μm and a depth of 40μm in about 30 minutes (25°C, 60% RH). The water-plastic polymer material becomes soft and plastic after being soaked in 50°C hot water for 30 minutes. The water-plastic polymer material also shows good recycling and reprocessing capabilities, and the mechanical strength of the recycled and reprocessed water-plastic polymer material is basically unchanged from the initial state.

[0066] Example 3

[0067] 15 g of bleached conifer pulp (Shijiazhuang Tengbang Mineral Products Co., Ltd.) was added to 1000 mL of deionized water and dispersed evenly by stirring, and 2 g of sodium bromide and 0.2 g of 2,6,6-tetramethylpiperidin-1-oxyl free radical were added and stirred evenly at room temperature; then 45 mL of sodium hypochlorite solution (with an effective chlorine content of 15 wt%) was dripped into the above system at a rate of 30 drops / min using a constant pressure funnel, and a 0.1 M NaOH solution was used to adjust the pH of the system to within the range of 10-10.2, and the reaction was carried out for 10 hours (including the dripping time of the sodium hypochlorite solution), the pH remained stable, and the reaction reached the oxidation endpoint; deionized water was used to wash until the filtrate pH was neutral and the ionic conductivity was less than 50 μS / cm, the slurry was collected and treated with a homogenizer to obtain a nanocellulose fiber dispersion, which was stored in a refrigerator at 4°C for use.

[0068] 2g N-(2-acryloyloxyethyl)-N-benzyl-N, N-dimethylammonium chloride (purchased from McLean), 4g methacrylic acid and 5g methyl polyethylene glycol acrylate monomethyl ether (purchased from Aladdin, average molecular weight 1000) were dissolved in 25g nanocellulose dispersion (solid content 1.5%), stirred for 20min, 0.18g 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (purchased from McLean) was added and mixed evenly, and three liquid nitrogen cooling-vacuuming-thawing cycles were performed, and then the obtained material was quickly (the operation was completed within 1 minute) poured into a polytetrafluoroethylene mold. The polymerization was carried out under ultraviolet irradiation for 1 hour (365nm exposure, average intensity 30mW cm -2 ) prepared water-plastic polymer materials based on ionic bond / hydrogen bond interactions.

[0069] The tensile strength of the water-plastic polymer material obtained above reaches 78.7MPa; the shape stability at room temperature and 90%RH is greater than 9 months. In about 35 minutes, a scratch with a width of 50μm and a depth of 20μm can be completely repaired (25℃, 60%RH); the water-plastic polymer material becomes soft and plastic after being soaked in 50℃ hot water for 30min. In addition, the tensile strength of the water-plastic polymer material after physical and chemical recycling exceeds that of common plastics on the market. The mechanical strength of the recycled and reprocessed water-plastic polymer material is basically unchanged from the initial state.

[0070] Example 4

[0071] 15 g of bleached conifer pulp (Shijiazhuang Tengbang Mineral Products Co., Ltd.) was added to 1000 mL of deionized water and dispersed evenly by stirring, and 2 g of sodium bromide and 0.2 g of 2,6,6-tetramethylpiperidin-1-oxyl free radical were added and stirred evenly at room temperature; then 45 mL of sodium hypochlorite solution (with an effective chlorine content of 15 wt%) was dripped into the above system at a rate of 30 drops / min using a constant pressure funnel, and a 0.1 M NaOH solution was used to adjust the pH of the system to within the range of 10-10.2, the reaction was carried out for 10 hours (including the dripping time of the sodium hypochlorite solution), the pH remained stable, and the reaction reached the oxidation endpoint; deionized water was used to wash until the filtrate pH was neutral and the ionic conductivity was less than 40 μS / cm, the slurry was collected and treated with a homogenizer to obtain a nanocellulose fiber dispersion, which was stored in a refrigerator at 4°C for use.

[0072] 2g of 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propionate, 5g of acrylic acid and 5g of methyl polyethylene glycol acrylate monomethyl ether were dissolved in 25g of nanocellulose dispersion (solid content 1%), stirred for 20min, and then 0.2g of methacryloyloxyethyl trimethylammonium chloride was added and mixed evenly, and then three liquid nitrogen cooling-vacuuming-thawing cycles were performed, and then the obtained material was quickly (completed within 1 minute) poured into a polytetrafluoroethylene mold. The polymerization was carried out by ultraviolet irradiation for 1 hour (365nm exposure, average intensity 30mW cm -2 ) prepared water-plastic polymer materials based on ionic bond / hydrogen bond interactions.

[0073] The tensile strength of the water-plastic polymer material prepared above is 82.9 MPa; the shape stability at room temperature and 90% RH is greater than 9 months. The water-plastic polymer material can completely repair a scratch with a width of 30 μm and a depth of 30 μm in about 25 minutes (25°C, 60% RH). The water-plastic polymer material becomes soft and plastic after being soaked in 50°C hot water for 30 minutes. The mechanical strength of the recycled water-plastic polymer material is basically unchanged from the initial state.

Claims

1. A water-plastic polymer material based on ionic bond / hydrogen bond interaction, characterized in that: Its general structural formula is: Wherein, a, b and c are positive integers, and 1≤a≤1000, 1≤b≤1000, 1≤c≤1000; a:b:c=(1-10):(10-1):(10-1); R1 is: any one of -COOH and -CH2COOH; R2 is: any one of -H or -CH3; R3 is: any one of -H or -CH3; R4 is: or Any of the following: R5 is: any one of -H or -CH3; R6 is: any one of -H or -CH2CH; The water-plastic polymer material based on ionic bond / hydrogen bond interaction is prepared by polymerization of nanocellulose fibers with quaternary ammonium salt acrylate monomers, acrylic acid-based monomers and polyethylene glycol acrylate monomers.

2. A method for preparing a water-plastic polymer material based on ionic bond / hydrogen bond interaction according to claim 1, characterized in that: The steps include: a. Using bleached conifer pulp as raw material, catalytic oxidation by 2,2,6,6-tetramethylpiperidinyl oxide was performed to prepare a nanocellulose fiber dispersion; b. The nanocellulose fiber dispersion obtained in step a is uniformly mixed with quaternary ammonium salt acrylate monomer, acrylic acid-based monomer and polyethylene glycol acrylate monomer, and a water-plastic polymer material is prepared by ultraviolet light curing polymerization.

3. The preparation method according to claim 2, characterized in that: Step a is: mixing sodium bromide, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, deionized water and bleached conifer pulp at room temperature, adding sodium hypochlorite solution, adjusting the pH to within the range of 10-10.2 with an alkaline solution, reacting until the pH is stable, washing with solvent 1 until the filtrate pH is neutral and the ion conductivity is less than 50 μS / cm, collecting the slurry and treating it with a homogenizer to obtain a nanocellulose fiber dispersion.

4. The preparation method according to claim 3, characterized in that: In step a, the mass ratio of sodium bromide to 2,2,6,6-tetramethylpiperidin-1-oxyl free radical is (8-10): (0.8-10); the ratio of the mass g of bleached conifer pulp to the volume mL of sodium hypochlorite solution is (0.5-1): (2.5-3.5); solvent 1 is at least one of deionized water or ethanol.

5. The preparation method according to any one of claims 2 to 4, characterized in that: Step b is: dissolving quaternary ammonium salt acrylate monomer, acrylic acid monomer and polyethylene glycol acrylate monomer in nanocellulose dispersion, stirring for 10 to 20 minutes, adding 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone and mixing evenly, degassing, and then pouring into a polytetrafluoroethylene mold, polymerizing under ultraviolet irradiation for 1 to 2 hours to obtain a water-plastic polymer material based on ionic bond / hydrogen bond interaction.

6. The preparation method according to claim 5, characterized in that: In step b, the acrylic acid-based monomer is at least one of acrylic acid and methacrylic acid; the polyethylene glycol acrylate monomer is at least one of methacrylate polyethylene glycol methacrylate, polyethylene glycol acrylate monomethyl ether or polyethylene glycol diacrylate; the quaternary ammonium salt acrylate monomer is at least one of acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, N-(2-acryloyloxyethyl)-N-benzyl-N,N-dimethylammonium chloride or 3-[[2-(methacryloyloxy)ethyl]dimethylammonium] propionate; the mass ratio of the quaternary ammonium salt acrylate monomer, the acrylic acid-based monomer, the polyethylene glycol acrylate monomer and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone is (0.30-1.55):(4.0-15.5):(4.0-15.5):(0.01-0.20).

7. The preparation method according to any one of claims 2 to 4, characterized in that: In step b, the mass ratio of the total mass of the quaternary ammonium salt acrylate monomer, the acrylic acid monomer and the polyethylene glycol acrylate monomer to the nanocellulose dispersion is (0.5-5.0):(10-50); the solid content of the nanocellulose dispersion is 1-2%.

8. A method for recycling water-plastic polymer materials based on ionic bond / hydrogen bond interaction according to claim 1, characterized in that: Cut the waste materials into pieces of 0.1-5 mm 2 , flatten, and hot press at a temperature of 35~40℃ and a pressure of 2~3MPa for 0.5~1h; or, cut the waste materials into pieces of 0.1~5mm 2 , immersed in water, add ammonium carbonate aqueous solution, react at 70-80°C for 1-2 hours, pour into a polytetrafluoroethylene mold, and dry and solidify; wherein the mass ratio of waste materials, water and ammonium carbonate aqueous solution is: (0.1-5.0): (10-50): (1-10).

9. An application of the water-plastic polymer material based on ionic bond / hydrogen bond interaction according to claim 1, characterized in that: Used to replace plastic.

Citation Information

Patent Citations

  • Preparation method of plant polyphenol / nanocellulose polymer composite material based on multi-hydrogen bond interaction

    CN108264743A

  • Preparation method and application method of TEMPO nanocellulose-polyacrylic acid gel

    CN109705370A

  • Redispersible nanocellulose composite material, preparation method and application

    CN117229572A

  • Cellulose dispersion composition and cellulose resin composite material

    JP2022051784A