A solidification method for waste incineration fly ash
The preparation of oligomer cement materials by incineration of fly ash and bottom ash for curing treatment is solved, and the problems of high cost and high resource consumption in traditional methods are achieved, and the stable curing and resource conservation of fly ash and bottom ash for waste incineration are achieved, which improves the Efficiency and resource utilization of garbage disposal.
Patent Information
- Application Number
- CN202410687163.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-30
AI Technical Summary
The existing waste incineration fly ash curing method is costly and consumes a lot of resources, especially the use of cement and chelating agents, and a low-cost and resource-saving treatment method is urgently needed.
Oligomeric cement materials are prepared by using fly ash and bottom ash generated during waste incineration, and the geopolymer materials are prepared by mixing and melting at high temperature, and curing them with an exciter to replace traditional cement and chelating agents.
The stable curing of waste incineration fly ash and bottom ash is achieved, cement and chelating agent resources are saved, and the efficiency and resource utilization of waste treatment are improved, and the curing effect is better than some traditional methods.
Smart Images

Figure CN118359392B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solid waste resource utilization, and in particular relates to a solidification method for waste incineration fly ash. Background Art
[0002] With the development of my country's economy, the improvement of people's living standards, the increase in per capita consumption of living materials, and the increase in the output of urban domestic waste, the annual growth rate is 8-10%. At present, the main methods of domestic waste treatment in my country are landfill, incineration and composting. Among them, incineration treatment has gradually become the main way to treat domestic waste due to its advantages of high reduction in volume and volume, and the heat generated by combustion can be utilized.
[0003] After the garbage is incinerated, ash is obtained, which is divided into two types of solid waste: bottom ash and fly ash. Bottom ash is the incineration residue discharged from the tail end of the furnace bed. The specific content is related to the type of garbage, the type of incinerator, the incineration conditions, etc. Fly ash is fine particles collected by the flue gas purification system equipment, generally collected by cyclone dust collectors, electrostatic dust collectors or bag dust collectors. The ash produced by the grate incinerator accounts for 15~20% of the incineration of domestic waste, of which fly ash accounts for 3~5% of the incineration of domestic waste, and bottom ash accounts for about 95% of the ash; the ash produced by the fluidized bed incinerator accounts for about 20~25% of the incineration of domestic waste, of which fly ash accounts for more than 10% of the incineration of domestic waste, and bottom ash accounts for about 80% of the ash.
[0004] Fly ash from garbage incineration is defined as hazardous waste because it contains pollutants generated by garbage incineration, mainly inorganic salts, heavy metals and dioxins. Incineration fly ash must be specially managed and disposed of. Compared with fly ash, bottom ash has the characteristics of diverse and complex material composition and low toxicity, and can be treated as general solid waste. Generally, bottom ash is a non-toxic and harmless waste according to China's current standards and can be used for paving roads, filling pits, and stacking.
[0005] At present, the main technology for handling fly ash in my country is to solidify and stabilize the fly ash from garbage incineration and then landfill it. The current solidification and stabilization technologies include cement solidification and stabilization technology, chelating agent solidification and stabilization technology, and cement-chelating agent combined solidification and stabilization technology. These three technologies use cement and chelating agents, which are relatively expensive and consume resources such as cement and chelating agents. Therefore, it is urgent to provide a solidification method for garbage incineration fly ash with low cost and low resource consumption. Summary of the invention
[0006] The purpose of the present invention is to provide a solidification method for waste incineration fly ash. The present invention utilizes two solid wastes, fly ash and bottom ash, generated in the waste incineration process to prepare oligomer cement material, which replaces cement and chelating agent to solidify the waste incineration fly ash. This not only solves the problem of fly ash and bottom ash in waste incineration plants, saves resources, but also provides a new path for the treatment of fly ash and bottom ash generated in the waste incineration process.
[0007] A solidification method for waste incineration fly ash of the present invention adopts the following technical scheme:
[0008] A solidification method for waste incineration fly ash comprises the following steps: uniformly mixing the geopolymer material, waste incineration fly ash and an activator with a water-cement ratio of 0.4 to 0.7 to obtain a solidified body.
[0009] Preferably, the mass percentages of the geopolymer material, waste incineration fly ash and activator are 35-55%, 40-60% and 0-10% respectively.
[0010] Preferably, the geopolymer material is prepared by melting waste incineration fly ash and waste incineration bottom ash.
[0011] Further preferably, the geopolymer material is prepared by the following steps: waste incineration fly ash and waste incineration bottom ash are produced by a grate furnace process and / or a fluidized bed process.
[0012] More preferably, the geopolymer material is prepared by the following steps: a mixture obtained by mixing waste incineration fly ash and waste incineration bottom ash is melted at high temperature, cooled naturally or by water quenching to obtain a geopolymer material block, and then the geopolymer material block is finely ground to obtain the geopolymer material.
[0013] Still further preferably, during the preparation of the geopolymer material, the mass percentage of waste incineration fly ash is 30-50%, and the mass percentage of waste incineration bottom ash is 50-70%.
[0014] Still more preferably, the high temperature melting temperature is 1000-1350° C., and the melting time is 40-180 min.
[0015] Preferably, the activator is NaOH, Ca(OH) 2 , water glass or at least one of the following.
[0016] Further preferably, the geopolymer block is finely ground using a ball mill or a rod mill to a mass fraction of -45µm ≥ 75% and a specific surface area ≥ 450m 2 / kg, and the geopolymer material is obtained.
[0017] Further preferably, the main elements of the waste incineration fly ash are as follows: Ca 25-45%, Si 1-10%, Cl 10-30%, Na 5-20%, K 2-10%, C 2-15%; the waste incineration fly ash also includes the following heavy metal elements in percentage by weight: Zn 0-1%, Pb 0-1%, Cu 0-1%, Ni 0-1%, Cr 0-1%, Cd 0-1%; the main components of the waste incineration bottom ash are as follows: CaO 2-15%, SiO 2 30~50%,Al 2 O 3 10~30%.
[0018] Beneficial effects:
[0019] The present invention utilizes two kinds of solid wastes, fly ash and bottom ash, generated during the incineration of garbage to prepare oligomer materials, and replaces cement and chelating agent in the solidification and stabilization process to solidify and stabilize the fly ash of the garbage incineration. It not only solves the problem of fly ash and bottom ash in the garbage incineration plant, but also saves resources such as cement and chelating agent, and realizes the maximum treatment and utilization of domestic garbage. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a flow chart of Example 1 of the present invention. DETAILED DESCRIPTION
[0021] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0022] Example 1
[0023] A method for solidifying fly ash from garbage incineration comprises the following steps:
[0024] (1) 30% by mass of waste incineration fly ash and 70% by mass of waste incineration bottom ash were mixed evenly and placed in a muffle furnace. The mixture was melted at 1350°C for 40 min. The melt was then taken out of the muffle furnace and quenched with water to obtain a geopolymer material block.
[0025] (2) Grind the geopolymer block to -45µm with a mass fraction of 76.45% and a specific surface area of 459m 2 / kg to obtain a geopolymer material powder, which is an amorphous material composed of silicon oxide tetrahedron and aluminum oxide tetrahedron.
[0026] (3) After mixing 35% by mass of geopolymer material powder, 55% by mass of waste incineration fly ash and 10% by mass of water glass with a water-cement ratio of 0.7, a solidified body is formed. The solidified body is used to prepare solidified body test blocks using a standard triple mold. The compressive strength of the solidified body is 3 MPa after 3 days and 7 MPa after 28 days. The solidified body is subjected to a toxicity leaching test according to the standard "Toxic Leaching Method of Solid Waste Leaching - Acetic Acid Buffer Solution Method" (HJ / T300-2007). The results are shown in Table 1. As can be seen from Table 1, the heavy metals Pb, Zn, Cu, Cd, Cr, As, etc. are all lower than the toxicity standard "Landfill Pollution Control Standard" (GB 16889-2008), indicating that the solidification effect is very good. The process is as follows Figure 1 shown.
[0027] The main elements of waste incineration fly ash are as follows: Ca 28%, Si 3%, Cl 25%, Na 11%, K 9%, C 5%; waste incineration fly ash also includes the following mass percentages of heavy metal elements: Zn 0.47%, Pb 0.21%, Cu 0.08%, Ni0.03%, Cr 0.11%, Cd 0.01%.
[0028] The main components of waste incineration bottom ash are as follows: CaO 6%, SiO 2 33%, Al 2 O 3 25%.
[0029] Example 2
[0030] A method for solidifying fly ash from garbage incineration comprises the following steps:
[0031] 50% by mass of waste incineration fly ash and 50% by mass of waste incineration bottom ash were mixed evenly and placed in a muffle furnace, melted at 1050°C for 180 minutes, and then the melt was taken out of the muffle furnace and naturally cooled to obtain a geopolymer material block. The geopolymer material block was finely ground to -45µm with a mass fraction of 83.57% and a specific surface area of 493m 2
[0032] / kg of geopolymer material powder, which is an amorphous material composed of silicon oxide tetrahedron and aluminum oxide tetrahedron. After mixing 55% of the mass fraction of geopolymer material powder and 45% of the mass fraction of garbage incineration fly ash, the water-cement ratio is 0.5 to form a solid body, and the solid body is used to prepare a solid body test block using a standard triple mold. The compressive strength of the solid body is 15Mpa after 3 days and 37Mpa after 28 days. The solid body is subjected to a toxicity leaching test, and the toxicity leaching test refers to the standard "Solid Waste Leaching Toxicity Leaching Method Acetic Acid Buffer Solution Method" (HJ / T300-2007), and the results are shown in Table 1. As can be seen from Table 1, heavy metals such as Pb, Zn, Cu, Cd, Cr, and As are all lower than the toxicity standard "Landfill Pollution Control Standard" (GB 16889-2008), indicating that the solidification effect is very good. The main elements of waste incineration fly ash are as follows: Ca 41%, Si 8%, Cl 15%, Na 16%, K 5%, C9%; waste incineration fly ash also includes the following mass percentages of heavy metal elements: Zn 0.43%, Pb 0.31%, Cu 0.06%, Ni 0.02%, Cr 0.04%, Cd 0.05%.
[0033] The main components of waste incineration bottom ash are as follows: CaO 11%, SiO 2 42%,Al 2 O 3 18%.
[0034] Example 3
[0035] A method for solidifying fly ash from garbage incineration comprises the following steps:
[0036] 40% by mass of waste incineration fly ash and 60% by mass of waste incineration bottom ash were mixed evenly and placed in a muffle furnace, melted at 1200°C for 90 minutes, and then the melt was taken out of the muffle furnace and water quenched to obtain a geopolymer material block. The geopolymer material block was finely ground to -45µm with a mass fraction of 83.45% and a specific surface area of 513m 2 / kg of geopolymer material powder, which is an amorphous material composed of silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron. After mixing 45% of geopolymer material powder, 50% of waste incineration fly ash, 3% of water glass and 2% of NaOH, the water-cement ratio is 0.4 to form a solid body, and the solid body is used to prepare solid body test blocks using a standard triple mold. The compressive strength of the solid body is 8Mpa after 3 days and 25Mpa after 28 days. The solid body is subjected to a toxicity leaching test, and the toxicity leaching test refers to the standard "Solid Waste Leaching Toxicity Leaching Method Acetic Acid Buffer Solution Method" (HJ / T300-2007), and the results are shown in Table 1. As can be seen from Table 1, heavy metals such as Pb, Zn, Cu, Cd, Cr, and As are all lower than the toxicity standard "Landfill Pollution Control Standard" (GB 16889-2008), indicating that the solidification effect is very good. The main elements of the waste incineration fly ash are as follows: Ca 33%, Si 5%, Cl 21%, Na 13%, K 4%, C 12%. The waste incineration fly ash also includes the following heavy metal elements in percentage by mass: Zn 0.37%, Pb 0.25%, Cu 0.07%, Ni 0.03%, Cr 0.07%, Cd 0.05%.
[0037] The main components of waste incineration bottom ash are as follows: CaO 4%, SiO 2 45%,Al 2 O 3 11%.
[0038] Table 1 Leaching toxicity results (unit: mg / L)
[0039]
[0040] Table 2 Leaching toxicity results (unit: mg / L)
[0041]
[0042] The fly ash in Example 1 was solidified and stabilized by cement, chelating agent and chelating agent-cement combined solidification, and the measured leaching toxicity results are shown in Table 2. As shown in Table 2, the solidification effect of the invention patent is better than that of the chelating agent solidification, and is similar to the solidification effect of cement solidification and combined solidification.
[0043] The present invention utilizes two kinds of solid wastes, fly ash and bottom ash, generated during the incineration of garbage to prepare oligomer cement materials, and replaces cement and chelating agent in the solidification and stabilization process to solidify and stabilize the fly ash of garbage incineration, thereby solving not only the problem of fly ash in garbage incineration plants, but also the problem of bottom ash, and realizing efficient resource utilization and maximum treatment of domestic garbage.
[0044] In the present invention, the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0045] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for solidifying fly ash from garbage incineration, It is characterized in that The geopolymer material, waste incineration fly ash and activator are mixed evenly with a water-cement ratio of 0.4 to 0.7 to obtain a solidified body; The geopolymer material is prepared by melting waste incineration fly ash and waste incineration bottom ash; the preparation of the geopolymer material adopts the following steps: melting the mixture obtained by mixing waste incineration fly ash and waste incineration bottom ash at high temperature, cooling naturally or water quenching to obtain a geopolymer material block, and then finely grinding the geopolymer material block to obtain the geopolymer material; the high temperature melting temperature is 1000-1200°C, and the melting time is 40-180min; The geopolymer material is an amorphous material composed of silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron; it replaces cement and chelating agent in the solidification and stabilization process to solidify and stabilize the waste incineration fly ash; The main elements of the waste incineration fly ash are as follows: Ca 25-45%, Si 1-10%, Cl 10-30%, Na 5-20%, K 2-10%, C 2-15%; the main components of the waste incineration bottom ash are as follows: CaO 2-15%, SiO 2 30~50%,Al 2 O 3 10-30%; The mass percentages of the geopolymer material, the waste incineration fly ash and the activator are 35-55%, 40-60% and 0-10% respectively.
2. The solidification method of waste incineration fly ash according to claim 1, It is characterized in that The geopolymer material is prepared by the following steps: waste incineration fly ash and waste incineration bottom ash are produced by a grate furnace process and / or a fluidized bed process.
3. The solidification method of waste incineration fly ash according to claim 1, It is characterized in that During the preparation of the geopolymer material, the mass percentage of waste incineration fly ash is 30-50%, and the mass percentage of waste incineration bottom ash is 50-70%.
4. The solidification method of waste incineration fly ash according to claim 1, It is characterized in that The activator is NaOH, Ca(OH) 2 , water glass or at least one of the following.
5. The solidification method of waste incineration fly ash according to claim 4, It is characterized in that Grind the geopolymer block with a ball mill or rod mill to a mass fraction of -45µm ≥ 75% and a specific surface area ≥ 450m 2 / kg, and the geopolymer material is obtained.
6. The solidification method of waste incineration fly ash according to claim 1, It is characterized in that The waste incineration fly ash also includes the following heavy metal elements in percentage by mass: Zn 0-1%, Pb 0-1%, Cu 0-1%, Ni 0-1%, Cr 0-1%, and Cd 0-1%.
Citation Information
Patent Citations
Garbage incineration ash slag heavy metal solidifying method
CN109516700A
Method for solidifying heavy metals in waste incineration fly ash
CN115368104A