Binder composition, pole piece and secondary battery
By using a multi-component copolymer containing -COOM groups and nitroaniline groups as the binder composition, the problem of low Li+ transmission rate in lithium-ion batteries in the existing technology is solved, and the ionic conductivity and ionic conductivity of lithium-ion batteries are improved. rate performance and simplifies the process.
Patent Information
- Application Number
- CN202410879743.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-02
AI Technical Summary
The existing composite system binder composition of styrene-butadiene rubber and carboxymethyl cellulose reduces the Li+ transmission rate of lithium-ion batteries and affects the cycle and rate performance of the battery.
A multi-component copolymer containing -COOM group and nitroaniline group is used as the binder composition, and is generated through the combined reaction of vinyl monomers, acrylate monomers and nitroaniline-containing monomers. Polymers with high ionic conductivity improve Li+ transmission speed and cycle performance of lithium-ion batteries.
Significantly improves the ion conductivity and rate performance of lithium-ion batteries, enhances the bonding force between the binder and the current collector, and has good flexibility, simplifying the process and avoiding the complexity of mixing different binders. .
Smart Images

Figure CN118406448B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a binder composition, a pole piece and a secondary battery. Background Art
[0002] As an energy storage device, lithium-ion batteries have the advantages of high energy, low cost, good safety performance and long cycle life. They are widely used in electric vehicles (EVs), plug-in hybrid electric vehicles (PHEVs) and portable electronic devices. With the popularization of lithium battery applications, people's demand for fast charging is becoming increasingly strong. How to improve the Li-ion battery during the charging and discharging process? + The transfer rate of Li will be one of the key points and hot spots of research. + It is necessary to migrate inside the crystals of the electrode active material particles, at the grain boundaries, and at the interface between the particle surface and the binder, conductive agent, and electrolyte to achieve Li + The transport of ions in the solid phase and between solid phases is a key step in limiting battery kinetics. Therefore, improving Li + The transmission rate within and between solid phases is one of the important methods to improve the working efficiency, energy density and power density of lithium-ion batteries.
[0003] Binder is an important component of the positive and negative electrodes of lithium-ion batteries. It adheres the electrode active material and conductive agent to the current collector in a small amount. Its main function is to bind and maintain the active material, stabilize the structure of the electrode, and buffer the expansion / contraction of the electrode during charging and discharging. It plays an important role in improving the cycle stability of the battery. The binder swells after absorbing the electrolyte, which can help the Li + The existing battery uses a composite system of styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) as a binder composition to improve some performance, but the composite system does not have ion transport properties, so it is not conducive to the battery's Li + The transmission rate of Li+ decreases, thereby reducing the cycle and rate performance of the battery. Therefore, a new type of binder composition is urgently needed to improve the Li+ + The transmission efficiency of ions can be improved, thereby improving the battery's rate, cycle and other performance. Summary of the invention
[0004] The technical problem to be solved by the present invention is that the existing binder composition of styrene-butadiene rubber and carboxymethyl cellulose as a composite system reduces the Li + To solve the problem of transmission rate, the present invention provides a binder composition, a pole piece and a secondary battery.
[0005] In order to solve the above technical problems, the present invention provides an adhesive composition, wherein the polymer contained in the adhesive composition comprises a vinyl structural unit, a (meth)acrylate structural unit and a functional structural unit; the functional structural unit comprises a structural unit represented by formula (I), formula (II) and / or formula (III),
[0006] (I) (II) (III),
[0007] Among them, R 1 , R 2 , R 3 are each independently selected from hydrogen or C 1-3 Alkyl, M is hydrogen or an alkali metal ion.
[0008] Preferably, the negative binder composition is obtained by reacting a raw material composition comprising a vinyl monomer, a (meth)acrylate monomer, a (meth)acrylic acid monomer, a nitroaniline-containing monomer, and an alkali metal compound.
[0009] Preferably, the weight ratio of the vinyl monomer, the (meth)acrylate monomer, the (meth)acrylic acid monomer, the nitroaniline-containing monomer and the alkali metal compound is 20-60:5-35:20-60:5-35:2-15.
[0010] Preferably, the weight ratio of the vinyl monomer, the (meth)acrylate monomer, the (meth)acrylic acid monomer, the nitroaniline-containing monomer and the alkali metal compound is 30-50:10-30:30-50:10-30:5-10.
[0011] Preferably, the (meth) acrylic monomer includes one or more of acrylic acid, methacrylic acid, ethacrylic acid, and propylacrylic acid;
[0012] And / or, the acrylic acid ester monomer includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, and sulfopropyl methacrylate.
[0013] Preferably, the nitroaniline-containing monomer includes one or more of 4-(3-nitroaniline)-4-oxo-2-butyric acid, acrolein-2,4-dinitrophenylhydrazone, and N-(3-nitroanilino)acrylamide.
[0014] Preferably, the ionic conductivity of the binder composition is 7×10 -4 -10×10 -4 S / cm.
[0015] In a second aspect, the present application provides a pole piece, comprising a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material, a negative electrode conductive agent, a thickener and the above-mentioned binder composition. Preferably, the peel strength of the pole piece is greater than 11N / m.
[0016] In a third aspect, the present application provides a secondary battery, comprising the above-mentioned electrode.
[0017] Compared with the existing technology, the adhesive composition provided by the present application has the following beneficial effects:
[0018] 1) The binder composition provided in the present application is a multi-polymer containing a -COOM group and a nitroaniline group, wherein the copolymer has a saturated carbon chain as the main chain. When the binder composition is applied to a lithium-ion battery, M is selected from Li + , the -COOLi contained in the side chain can dissociate to produce Li + , so that the binder becomes a conductive polymer under the action of the electric field, which greatly improves the ionic conductivity of the lithium-ion battery and can improve Li + At the same time, the side chain has a strong electron-withdrawing -NO 2 Under the strong electron-withdrawing effect, electrons tend to migrate to the vicinity of the nitro group, thus constructing a specific Li + Migration channel, -NH group can interact with anions containing lone pair electrons in the electrolyte to form hydrogen bonds, which is beneficial to the Li + dissociation, which increases the ionic conductivity and improves the Li + The transmission speed is improved to improve the rate performance of lithium-ion batteries. Similarly, when the binder composition is applied to sodium-ion batteries, M is selected from Na + , the -COONa contained in the polymer side chain can dissociate into Na + , it can also improve the ionic conductivity of sodium ion batteries and increase the Na + The transmission rate.
[0019] 2) The multi-polymer containing -COOM groups contains carboxyl groups, which can improve the bonding force between the binder and the current collector and improve the cycle performance of lithium-ion batteries.
[0020] 3) The binder composition provided in the present application is used in batteries to improve the transmission rate of lithium ions, and also has good flexibility. In specific applications, there is no need to mix the binder composition provided in the present application with other binders, thus avoiding the process complexity caused by the current mixing of different types of binders.
[0021] 4) After the binder composition provided in the present application swells the electrolyte, the ionic conductivity is tested to be 7×10 -4 ~10×10 -4 S / cm, and the binder composition has a higher ionic conductivity after swelling the electrolyte. DETAILED DESCRIPTION
[0022] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0023] On the one hand, an embodiment of the present application provides an adhesive composition, wherein the polymer contained in the adhesive composition includes a vinyl structural unit, an acrylate structural unit and a functional structural unit; the functional structural unit contains a structural unit as shown in formula (I), formula (II) and / or formula (III),
[0024] (I) (II) (III),
[0025] Among them, R 1 , R 2 , R 3 are each independently selected from hydrogen or C 1-3 Alkyl, M is hydrogen or an alkali metal ion.
[0026] In specific applications, the functional structural unit contains structural units as shown in formula (I) and formula (II), or the functional structural unit contains structural units as shown in formula (I) and formula (III), or the functional structural unit contains structural units as shown in formula (I), formula (II) and formula (III).
[0027] Preferably, the -COOM-containing structural unit is obtained by reacting an acrylic structural unit with an alkali metal compound.
[0028] Compared with the existing technology, the adhesive composition provided by the present application has the following beneficial effects:
[0029] 1) The binder composition provided in the present application is a multi-polymer containing a -COOM group and a nitroaniline group, wherein the copolymer has a saturated carbon chain as the main chain. When the binder composition is applied to a lithium-ion battery, M is selected from Li + , the -COOLi contained in the side chain can dissociate to produce Li + , so that the binder becomes a conductive polymer under the action of the electric field, which greatly improves the ionic conductivity of the lithium-ion battery and can improve Li + At the same time, the side chain has a strong electron-withdrawing -NO 2 Under the strong electron-withdrawing effect, electrons tend to migrate to the vicinity of the nitro group, thus constructing a specific Li + Migration channel, -NH group can interact with anions containing lone pair electrons in the electrolyte to form hydrogen bonds, which is beneficial to the Li + dissociation, which increases the ionic conductivity and improves the Li + The transmission speed is improved to improve the rate performance of lithium-ion batteries. Similarly, when the binder composition is used in sodium-ion batteries, M is selected from Na + , the -COONa contained in the polymer side chain can dissociate into Na + , it can also improve the ionic conductivity of sodium ion batteries and increase the Na + The transmission rate.
[0030] 2) The multi-polymer containing -COOM groups contains carboxyl groups, which can improve the bonding force between the binder and the current collector and improve the cycle performance of lithium-ion batteries.
[0031] 3) The binder composition provided in the present application is used in batteries to improve the transmission rate of lithium ions, and also has good flexibility. In specific applications, there is no need to mix the binder composition provided in the present application with other binders, thus avoiding the process complexity caused by the current mixing of different types of binders.
[0032] 4) After the binder composition provided in the present application swells the electrolyte, the ionic conductivity is tested to be 7×10 -4 ~10×10 -4 S / cm, and the binder composition has a higher ionic conductivity after swelling the electrolyte.
[0033] Specifically, the preparation method of the polymer is preferably emulsion polymerization, such as emulsion polymerization of vinyl monomers, acrylic monomers, acrylate monomers and monomers containing nitroaniline groups, which can generate a binder composition of a multi-polymer containing nitroaniline groups.
[0034] In some embodiments, the weight ratio of the vinyl monomer, the (meth)acrylate monomer, the (meth)acrylic acid monomer, the nitroaniline-containing monomer, and the alkali metal compound is 20-60:5-35:20-60:5-35:2-15.
[0035] Preferably, the weight ratio of the vinyl monomer, the acrylate monomer, the acrylic acid monomer, the monomer containing a nitroaniline group and the alkali metal compound is 30-50:10-30:30-50:10-30:5-10.
[0036] Preferably, the alkali metal compound is lithium hydroxide or sodium hydroxide.
[0037] When preparing the polymer, because it is a polymerization reaction, it is necessary to add an initiator, a surfactant and a solvent. The weight of the initiator added during the preparation of the polymer is 0.5 to 3 parts, the weight of the surfactant is 0.1 to 5 parts, and the weight of the solvent is 100 to 200 parts.
[0038] Vinyl monomers include styrene monomers, acrylic monomers include acrylic acid, and acrylate monomers include propyl acrylate. The reaction equation for the multi-polymer generated by taking vinyl monomers, acrylic acid, propyl acrylate, and N-(3-nitroanilino)acrylamide monomers as examples is as follows.
[0039] Equation 1:
[0040] .
[0041] Equation 2:
[0042] .
[0043] In the above equations 1 and 2, m 1 is the molar amount of the vinyl monomer, m 2 is the molar amount of acrylic acid monomer, m 3 is the molar amount of propyl acrylate monomer, m 4 is the molar amount of N-(3-nitroanilino)acrylamide monomer, and this application does not limit m 1 、m 2 、m 3 、m 4 range.
[0044] In equation 2, m 21 It is based on the molar amount of vinyl monomer in the reactants m 1 , molar amount of acrylic acid monomer m 2 Depending on the 21 ≤m 1+m 2 . m in Equation 2 3 、m 4 It is the degree of polymerization in the copolymer, which is related to the molar amount of the added propyl acrylate monomer and the molar amount of the N-(3-nitroanilino)acrylamide monomer.
[0045] It should be noted that the structural formula of the multi-polymer containing nitroaniline groups generated by emulsion polymerization of vinyl monomers, acrylic monomers, acrylate monomers and nitroaniline group-containing monomers can also be other structures, such as the vinyl structural unit is located between the acrylic structural unit and the acrylate structural unit, or the vinyl structural unit is located between the acrylate structural unit and the structural unit containing nitroaniline groups, or the vinyl structural unit is located between the acrylic structural unit and the structural unit containing nitroaniline groups.
[0046] Specifically, the weight of the vinyl monomer added during the polymer preparation process is 30-50 parts, and during the reaction, the vinyl monomers are polymerized with each other, or the vinyl monomers are polymerized with acrylic monomers, etc. During the preparation of the adhesive composition, the weight of the vinyl monomer added can be in the following ranges: 30-37 parts, 37-40 parts, 40-42 parts, 42-45 parts, 45-48 parts, 48-50 parts.
[0047] Specifically, the weight portion of acrylic monomer added during the polymer preparation process is 30 to 50 parts. When the binder composition is applied to lithium-ion batteries, the acrylic structural unit contains a carboxyl group, which can form a side chain containing -COOLi after reacting with lithium hydroxide. The dissociated Li + , improve the ionic conductivity of lithium-ion batteries, and can also improve the bonding force between the binder and the current collector, and improve the cycle performance of lithium-ion batteries; if the weight of the acrylic monomer added in the preparation of the binder composition is less than 30 parts, the weight of the acrylic structural unit in the formed polymer is less than 30 parts, and the carboxyl content of the generated polymer is reduced, affecting the bonding strength of the binder; if the weight of the acrylic monomer added in the preparation of the binder composition is greater than 50 parts, the weight of the acrylic structural unit in the formed polymer is greater than 50 parts, and the glass transition temperature of the prepared binder composition is higher, and the brittleness increases. The weight of the acrylic monomer added in the preparation of the binder composition can be 30 parts, 32 parts, 35 parts, 38 parts, 40 parts, 42 parts, 45 parts, 48 parts, 50 parts, etc., as long as it is within the range of 30 to 50 parts.
[0048] In some embodiments, the acrylic monomer includes one or more of acrylic acid, methacrylic acid, hydroxypropyl acrylic acid, ethacrylic acid, and propyl acrylic acid.
[0049] Specifically, the weight portion of the acrylic ester monomer added during the preparation of the binder composition is 10 to 30 parts. The acrylic ester monomer contains an ester group. The prepared polymer contains an acrylic acid structural unit, which can provide an appropriate amount of -O- functional groups on the side chains for the multi-polymer. When the binder composition is applied to a lithium-ion battery, the -O- functional groups on the side chains can serve as coordination sites with Li + The polymer chains are continuously moving in situ to generate free volume. Under the action of the electric field, Li + Migrate from one coordination site to another along the polymer chain, or jump from one chain segment to another to achieve Li + At the same time, the good compatibility of esters with electrolyte solvents is conducive to the infiltration of electrolytes, which improves the Li + If the weight of the acrylate monomer is too low, the content of the acrylate structural unit of the prepared polymer will be reduced, and the side chain of the generated copolymer will contain fewer -O- functional groups, and Li + The transmission speed is reduced, affecting the rate performance of the lithium-ion battery. If the weight of the acrylic acid ester monomer is too high, the swelling of the binder in the electrolyte is too large, which will affect the cycle performance of the battery. Specifically, the weight of the acrylic acid ester monomer added during the preparation of the binder composition can be 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts, 30 parts, etc., as long as it is within the range of 10 to 30 parts.
[0050] In some embodiments, the acrylic acid ester monomer includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, and sulfopropyl methacrylate.
[0051] Specifically, the weight portion of the monomer containing nitroaniline groups added during the preparation of the adhesive composition is 10 to 30 parts, and the resulting adhesive composition is a multi-polymer containing nitroaniline groups, and the side chain contains a -NO with strong electron-withdrawing 2 Under the strong electron-withdrawing effect, electrons tend to migrate to the vicinity of the nitro group, thus constructing a specific Li + Migration channel, -NH group can interact with anions containing lone pair electrons in the electrolyte to form hydrogen bonds, which is beneficial to the Li + dissociation, which increases the ionic conductivity and improves the Li + The transmission speed is improved, and the rate performance of lithium-ion batteries is improved.
[0052] In the preparation process of the binder composition, if the weight of the monomer containing the nitroaniline group is less than 10 parts, the -NO 2 The -NH group and -NH group are reduced, the transfer rate of lithium ions in the binder composition is reduced, and the rate performance of the battery is reduced. If the weight of the monomer containing the nitroaniline group is higher than 30 parts, the types of other monomers are reduced, which affects the migration rate of lithium ions and the rate performance and cycle performance of the lithium ion battery. Specifically, the weight of the monomer containing the nitroaniline group in the binder composition can be in the following ranges: 10-14 parts, 14-17 parts, 17-20 parts, 20-25 parts, 25-28 parts, 28-30 parts.
[0053] In some embodiments, the monomer containing a nitroaniline group includes one or more of 4-(3-nitroaniline)-4-oxo-2-butyric acid, acrolein-2,4-dinitrophenylhydrazone, and N-(3-nitroanilino)acrylamide.
[0054] In some preferred embodiments, the weight ratio of the vinyl monomer, the acrylate monomer, the acrylic acid monomer, the monomer containing the nitroaniline group and the alkali metal compound is 30-45:15-30:35-50:15-25:5-10. The binder composition prepared by using the raw materials with this weight ratio has a high swelling rate and good flexibility, which improves the peel strength of the negative electrode sheet and is more conducive to significantly improving the ionic conductivity of the lithium-ion battery and improving Li + The transmission speed can improve the battery rate performance, safety performance and cycle performance.
[0055] In some embodiments, the raw materials for preparing the adhesive composition include the following parts by weight: 30 to 45 parts of vinyl monomers, 30 to 50 parts of acrylic monomers, 15 to 30 parts of acrylate monomers, 15 to 25 parts of monomers containing nitroaniline groups, 0.5 to 2 parts of initiators, 0.5 to 3 parts of surfactants, and 100 to 150 parts of solvents.
[0056] Specifically, the binder composition prepared by using vinyl monomers, acrylic monomers, acrylate monomers, and monomers containing nitroaniline groups within the above range has a high swelling rate and good flexibility, which improves the peel strength of the negative electrode sheet and is more conducive to significantly improving the ionic conductivity of lithium-ion batteries and improving Li + The transmission speed can improve the battery rate performance, safety performance and cycle performance.
[0057] In some embodiments, the ionic conductivity of the binder composition is 7×10 -4 ~10×10 -4 S / cm.
[0058] Specifically, the ionic conductivity of the binder composition is 7×10 -4 ~10×10 -4 S / cm range, which helps to increase the transfer rate of lithium ions and improve the cycle performance and rate performance of the battery.
[0059] In some embodiments, the raw materials of the adhesive composition include 30 to 50 parts of styrene monomer, 30 to 50 parts of acrylic monomer, 10 to 30 parts of acrylate monomer, 10 to 30 parts of monomer containing nitroaniline group, 0.5 to 3 parts by weight of initiator, 0.1 to 5 parts by weight of surfactant, and 100 to 200 parts by weight of solvent.
[0060] In some embodiments, the initiator comprises a peroxide-based initiator;
[0061] The surfactant includes one or more of anionic surfactants, cationic surfactants, amphoteric surfactants and nonionic surfactants.
[0062] Specifically, the weight portion of the initiator is 0.5 to 3 parts, which has the function of initiating polymerization of vinyl monomers, acrylic monomers, acrylate monomers, and monomers containing nitroaniline groups, and can improve the reaction rate and efficiency. If the weight portion of the initiator is too low, the reaction rate is reduced; if the weight portion of the initiator is too high, the collision probability of free radicals is accelerated, the degree of polymerization is reduced, and the mechanical properties and bonding properties of the adhesive composition are reduced.
[0063] When surfactants are dissolved in a solution, they can significantly reduce the surface tension or interfacial tension of the solution and improve the solubilization, emulsification, and dispersion effects of the solution.
[0064] In some preferred embodiments, the initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate;
[0065] The surfactant includes one or more of sodium dodecyl sulfate, sodium octadecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene ether, polyoxypropylene ether, alcohol ether carboxylate, alcohol ether phosphate, triethanolamine dodecylbenzene sulfonate, octylphenol polyoxyethylene ether, and polyoxyethylene fatty acid ester.
[0066] In some embodiments, the alkali metal compound also has the function of a buffer to adjust the pH value, and adjusts the pH value of the binder composition to 5-9, and is used in lithium-ion batteries to prevent the acidity of the binder composition from increasing battery side reactions.
[0067] In some preferred embodiments, the alkali metal compound includes an alkaline compound containing lithium metal, and the binder composition prepared in this case can be used in lithium ion batteries, lithium metal batteries, etc.; the buffer can also be an alkaline compound containing sodium metal, and the binder composition prepared in this case can be used in sodium ion batteries.
[0068] It should be noted that the adhesive composition provided in the present application also has good mechanical properties and mechanical properties, and high stability.
[0069] In some preferred embodiments, the alkali metal compound includes lithium hydroxide or sodium hydroxide; and the solvent includes water.
[0070] In a second aspect, the present application provides an electrode sheet, comprising a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material, a negative electrode conductive agent, a thickener and the binder composition described above.
[0071] Specifically, the electrode sheet includes a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material layer is arranged on at least one side surface of the negative electrode current collector. The negative electrode current collector includes copper foil.
[0072] The negative electrode active material adopts existing ones, such as the negative electrode active material includes at least one of graphite, silicon element, and silicon-carbon material. The negative electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, and graphene.
[0073] The electrode provided in the present application has strong bonding properties using the above-mentioned binder composition, which enhances the bonding force between the negative electrode active material layer and the negative electrode current collector, increases the migration rate of lithium ions in the negative electrode active material layer, and improves the ionic conductivity and rate performance of the battery.
[0074] In some preferred embodiments, the thickener includes CMC (sodium carboxymethyl cellulose).
[0075] The adhesive composition provided in the present application has good bonding properties, and the prepared electrode has a peel strength greater than 11 N / m.
[0076] In a third aspect, the present application provides a secondary battery, comprising a positive electrode sheet and the electrode sheet described above.
[0077] Specifically, secondary batteries include lithium batteries, lithium ion batteries, lithium sulfur batteries, sodium ion batteries, etc. When the battery is a sodium ion battery, the alkali metal compound used in preparing the binder composition should be sodium hydroxide or an alkaline compound containing sodium ions.
[0078] The secondary battery provided in the present application uses the above-mentioned negative electrode sheet to improve the adhesion between the negative electrode active material layer and the negative electrode current collector, thereby improving the battery's cycle performance; at the same time, the above-mentioned binder composition is used to improve the battery's ion conductivity and ion migration rate, thereby improving the battery's rate performance.
[0079] In a fourth aspect, the present application provides a method for preparing the above-mentioned adhesive composition, comprising the following steps:
[0080] S1: uniformly mixing part of the solvent, the vinyl monomer, the acrylic monomer, the acrylate monomer and the monomer containing the nitroaniline group to obtain a pre-emulsion;
[0081] S2: adding another part of the solvent and the surfactant into the reaction kettle and mixing them evenly, then introducing a protective gas, heating to a first reaction temperature, adding part of the initiator and the pre-emulsion to carry out a polymerization reaction;
[0082] S3: After the polymerization reaction is completed, the mixture is heated to a second reaction temperature, another portion of the initiator is added for aging, and after the aging is completed, an alkali metal compound is added to adjust the pH to obtain the binder composition.
[0083] The preparation method of the binder composition provided in the present application has a simple process, and adopts emulsion polymerization to obtain a multi-copolymer binder composition, which has high mechanical strength and high bonding strength with the current collector, thereby improving the cycle performance of the lithium ion battery; the side chain of the copolymer contains a + The groups greatly improve the ionic conductivity of lithium-ion batteries and can increase the Li + The side chain has a coordination site that can be used as a Li + The -O-functional group for coupling realizes Li + migration, increasing the Li + The transmission speed of the lithium-ion battery is improved. 2 Under the strong electron-withdrawing effect, electrons tend to migrate to the vicinity of the nitro group, thus constructing a specific Li + Migration channel. The -NH group can interact with anions containing lone pair electrons in the electrolyte to form hydrogen bonds, which is beneficial to the Li + dissociation, which increases the ionic conductivity and improves the Li + The transmission speed is improved, and the rate performance of lithium-ion batteries is improved.
[0084] In some embodiments, the shielding gas includes nitrogen, a noble gas.
[0085] Further preferably, the protective gas includes high-purity nitrogen.
[0086] Specifically, the oxygen contained in the air in the reactor has an inhibitory effect, which causes the reaction induction period to become longer and reduces the polymerization efficiency in the polymerization reaction; introducing a protective gas such as high-purity nitrogen to replace the air in the reactor reduces the oxygen content in the reaction system and increases the reaction rate.
[0087] In some embodiments, the mass content of the partial solvent in step S1 accounts for 25% to 50% of the total solvent; the mass content of the partial initiator in step S2 accounts for 70% to 90% of the total initiator.
[0088] In some embodiments, in step S2, the first reaction temperature is 55-75° C., and the polymerization reaction time is 3-5 h.
[0089] Specifically, in step S2, a portion of the initiator and the pre-emulsion are added to carry out a polymerization reaction; wherein the polymerization reaction temperature is the same as the first reaction temperature, that is, the polymerization reaction is carried out at the first reaction temperature.
[0090] In some embodiments, in step S3, the second reaction temperature is 65-85° C., and the aging time is 2-4 hours.
[0091] Specifically, in step S3, after the polymerization reaction is completed, the mixture is heated to a second reaction temperature, and another portion of initiator is added for aging. The aging refers to aging at the second reaction temperature.
[0092] Specifically, after aging, the pH is adjusted to obtain the binder composition, wherein the pH is adjusted using an alkali metal compound, and the alkali metal compound includes lithium hydroxide or sodium hydroxide.
[0093] The present invention is further described below by way of examples.
[0094] The binder composition, negative electrode composition, negative electrode sheet and lithium ion battery disclosed in the present invention are specifically described.
[0095] Example 1
[0096] 1) Preparation of binder composition
[0097] S1: Mix part of the solvent, deionized water, surfactant, vinyl monomer, acrylic monomer, acrylate monomer and nitroaniline group-containing monomer, add them into a pre-emulsification kettle, start stirring for high-speed pre-emulsification to obtain a uniform pre-emulsified liquid, and transfer the pre-emulsified liquid to a constant pressure dropping funnel for standby use.
[0098] Among them, the mass content of partial solvent deionized water accounts for 25% of the total solvent deionized water;
[0099] The surfactant is sodium dodecyl sulfate, the acrylic monomer is methacrylic acid, the acrylic ester monomer is isobutyl acrylate, and the monomer containing nitroaniline group is N-(3-nitroanilino) acrylamide.
[0100] S2: Add another part of the solvent and surfactant into the reactor and mix them evenly, then introduce protective gas high-purity nitrogen to replace the air;
[0101] Then, the heating reactor was turned on, and stirring was performed while heating. When the temperature in the reactor reached the first reaction temperature of 60°C, part of the initiator was added. After the initiator was added, the constant pressure dropping funnel was turned on to start dropping the pre-emulsified liquid for reaction. During the reaction, stirring was turned on and nitrogen was passed. The stirring rate during the reaction was 100 r / min, and the polymerization reaction time was 4 hours.
[0102] Wherein, in step S2, the mass percentage of the partial initiator to the total initiator is 90%.
[0103] S3: After the polymerization reaction is completed, the temperature is continued to rise to the second reaction temperature of 70°C, another portion of the initiator is added, and the mixture is continuously stirred for heat preservation and aging, and nitrogen is continuously introduced during the aging process. During the aging process, the stirring rate is 100 r / min and the aging time is 3 hours.
[0104] After aging, the mixture is naturally cooled to room temperature, and then filtered to obtain a polymer emulsion. Buffering agent lithium hydroxide is added to the polymer emulsion to adjust the pH value to 5-9 to obtain a binder composition.
[0105] In the process of preparing the adhesive composition of Example 1, the polymer includes the following parts by weight: 30 parts of vinyl monomer, 30 parts of acrylic monomer, 10 parts of acrylate monomer, 10 parts of monomer containing nitroaniline group, 1 part of initiator, 1 part of surfactant, 6 parts of lithium hydroxide, and 120 parts of solvent.
[0106] Example 2
[0107] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 40 parts of vinyl monomer are used.
[0108] Example 3
[0109] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 42 parts of acrylic acid monomer.
[0110] Example 4
[0111] Most of the steps of this embodiment are the same as those of embodiment 1, except that 20 parts of the monomer containing nitroaniline group are used.
[0112] Example 5
[0113] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 22 parts of acrylic acid ester monomer are used.
[0114] Example 6
[0115] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 43 parts of vinyl monomer and 24 parts of acrylate monomer.
[0116] Example 7
[0117] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 47 parts of vinyl monomer, 26 parts of monomer containing nitroaniline group, 2 parts of initiator, 2 parts of surfactant, 6 parts of lithium hydroxide, and 150 parts of solvent.
[0118] Example 8
[0119] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 43 parts of acrylic acid monomer and 24 parts of acrylate monomer.
[0120] Example 9
[0121] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 48 parts of acrylic monomer, 30 parts of monomer containing nitroaniline group, 2.2 parts of initiator, 3.1 parts of surfactant, 6 parts of lithium hydroxide, and 160 parts of solvent.
[0122] Example 10
[0123] Most of the steps of this embodiment are the same as those of Embodiment 1, except that: 46 parts of vinyl monomer, 42 parts of acrylic monomer, 23 parts of acrylate monomer, 1.8 parts of initiator, 3.5 parts of surfactant, 7 parts of lithium hydroxide, and 145 parts of solvent.
[0124] Embodiment 11
[0125] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 46 parts of vinyl monomer, 42 parts of acrylic monomer, 30 parts of monomer containing nitroaniline group, 2.5 parts of initiator, 4.0 parts of surfactant, 8 parts of lithium hydroxide, and 180 parts of solvent.
[0126] Example 12
[0127] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 46 parts of vinyl monomer, 23 parts of acrylate monomer, 30 parts of monomer containing nitroaniline group, 2.6 parts of initiator, 4.2 parts of surfactant, 8.5 parts of lithium hydroxide, and 190 parts of solvent.
[0128] Embodiment 13
[0129] Most of the steps of this embodiment are the same as those of embodiment 1, except that: 48 parts of acrylic monomer, 23 parts of acrylate monomer, 30 parts of monomer containing nitroaniline group, 2.6 parts of initiator, 4.2 parts of surfactant, 8.5 parts of lithium hydroxide, and 190 parts of solvent.
[0130] Embodiment 14
[0131] Most of the steps of this embodiment are the same as those of Embodiment 1, except that: 50 parts of vinyl monomer, 50 parts of acrylic monomer, 30 parts of acrylate monomer, 30 parts of monomer containing nitroaniline group, 3 parts of initiator, 5 parts of surfactant, 9 parts of lithium hydroxide, and 200 parts of solvent.
[0132] Embodiment 15
[0133] Most of the steps of this embodiment are the same as those of embodiment 1, except that the types of surfactant, acrylic monomer, acrylate monomer and nitroaniline group-containing monomer are different, as described below.
[0134] The surfactant is alcohol ether carboxylate and alcohol ether phosphate;
[0135] The acrylic monomers are hydroxypropyl acrylate, ethyl acrylate and propyl acrylate;
[0136] Acrylate monomers are ethyl acrylate, ethyl methacrylate and propyl methacrylate;
[0137] The monomer containing nitroaniline group is a mixture of 4-(3-nitroaniline)-4-oxo-2-butyric acid, acrolein-2,4-dinitrophenylhydrazone and N-(3-nitroanilino)acrylamide.
[0138] Comparative Example 1
[0139] Most of the steps of this comparative example are the same as those of Example 1, except that: 0 part of vinyl monomer is used.
[0140] Comparative Example 2
[0141] Most of the steps of this comparative example are the same as those of Example 1, except that: 0 part of the monomer containing nitroaniline group is used.
[0142] Comparative Example 3
[0143] Most of the steps of this comparative example are the same as those of Example 1, except that: 10 parts of vinyl monomer are used.
[0144] Comparative Example 4
[0145] Most of the steps of this comparative example are the same as those of Example 1, except that: 60 parts of vinyl monomer are used.
[0146] Comparative Example 5
[0147] Most of the steps of this comparative example are the same as those of Example 1, except that 5 parts of the monomer containing nitroaniline group are used.
[0148] Comparative Example 6
[0149] Most of the steps of this comparative example are the same as those of Example 1, except that 38 parts of the monomer containing nitroaniline group are used.
[0150] Comparative Example 7
[0151] Most of the steps of this comparative example are the same as those of Example 1, except that: 2 parts of acrylic acid ester monomer are used.
[0152] Comparative Example 8
[0153] Most of the steps of this comparative example are the same as those of Example 1, except that: 40 parts of acrylic acid ester monomer.
[0154] Comparative Example 9
[0155] Most of the steps of this comparative example are the same as those of Example 1, except that: 20 parts of acrylic acid monomer.
[0156] Comparative Example 10
[0157] Most of the steps of this comparative example are the same as those of Example 1, except that: 62 parts of acrylic acid monomer.
[0158] Performance Test:
[0159] The binder compositions prepared in the above-mentioned embodiments and comparative examples were used to prepare negative electrode sheets and lithium-ion batteries according to the prior art, and the following tests were performed. The negative electrode sheet's negative electrode active material was graphite, the negative electrode conductive agent was conductive carbon black, and the thickener was CMC. The mass ratio of graphite, conductive carbon black, thickener, and binder composition was 96.8:1.0:1.2:1.0.
[0160] 1) Testing the ionic conductivity of the binder composition after swelling the electrolyte
[0161] The ionic conductivity of the binder composition prepared in the above embodiments and comparative examples after swelling the electrolyte was tested by using the electrochemical impedance spectroscopy (EIS) technique in an electrochemical workstation;
[0162] The test temperature is 25℃ and the test frequency is 10 -2 -10 5Hz, with an amplitude of 5 mV. The swollen adhesive composition film was placed between two stainless steel sheets and assembled into a CR2025 button cell for testing. In the Nyquist plot, the bulk resistance Re was measured.
[0163] The calculation formula of ionic conductivity is σ=d / (Re×S),
[0164] Where d is the film thickness and S is the area of the stainless steel sheet.
[0165] 2) Negative electrode peel strength test:
[0166] After the negative electrode sheet prepared above was compacted, the peel strength of the negative electrode sheet was measured using a tensile testing machine, and the test method was based on GB2792-2014.
[0167] 3) Normal temperature cycle test
[0168] The specific method is: let the soft pack battery stand until the temperature reaches 25℃±2℃, test the capacity of the soft pack battery, record it as the capacity before storage, discharge the soft pack battery at 0.5C constant current to 2.7V, charge at 1C constant current to 4.3V, then charge at constant voltage to the cut-off current of 0.05C, and then discharge at 1C constant current to 2.75V after charging is completed; cycle 500 times in this way and record the capacity retention rate.
[0169] 4) Rate performance test:
[0170] The batteries prepared in the above embodiments and comparative examples were discharged at a constant current of 0.5C to a voltage of 2.75V at a temperature of 25°C±2°C. They were then charged at a constant current of 1C to a voltage of 4.3V, and then charged at a constant voltage to a cut-off current of 0.05C. The fully charged battery was discharged at 1C, and the discharge capacity C1 of the battery was recorded. Thereafter, the battery was discharged at a constant current of 1C, 2C, and 3C to 2.75V, and the discharge capacity C2 of the battery was recorded.
[0171] Rate discharge capacity retention rate = C2 / C1 100%.
[0172] The test results of 1) to 4) above are shown in Table 1.
[0173] Table 1
[0174]
[0175] It can be seen from Table 1 that, by comparing Example 1 with Comparative Examples 1, 3 and 4, there is no vinyl monomer in the polymer, and the ionic conductivity and bonding performance of the binder composition are poor. When the weight portion of the styrene monomer is less than 30 parts, the ionic conductivity of the binder composition is even worse. When the weight portion of the styrene monomer is greater than 50 parts, although the ionic conductivity and bonding performance are improved, the rate performance of the battery is still poor. This indicates that when the weight portion of the vinyl monomer in the polymer is in the range of 30 to 50 parts, the ionic conductivity of the binder composition is high and the bonding performance is good, which is helpful to improve the rate performance of the battery. In comparison between Example 1 and Comparative Examples 2, 5, and 6, the polymer does not contain a monomer containing a nitroaniline group, the ionic conductivity of the binder composition is the lowest, and the rate performance of the battery is poor. When a monomer containing a nitroaniline group is added, but the amount added is not within the range of 10 to 30 parts, the bonding performance is poor, the capacity retention rate of the battery at different rates is still poor, and the cycle capacity retention rate is low, indicating that when the weight portion of the monomer containing a nitroaniline group added to the polymer is 10 to 30 parts, the side chain contains a -NO with a strong electron-withdrawing 2 Under the strong electron-withdrawing effect, electrons tend to migrate to the vicinity of the nitro group, thus constructing a specific Li + Migration channel. The -NH group can interact with anions containing lone pair electrons in the electrolyte to form hydrogen bonds, which is beneficial to the Li + dissociation, which increases the ionic conductivity and improves the Li + The transmission speed is improved, and the rate performance of lithium-ion batteries is improved.
[0176] Comparison between Example 1 and Comparative Examples 7 and 8, and between Example 1 and Comparative Examples 9-10, shows that 30-50 parts of acrylate monomers and 30-50 parts of acrylic acid monomers can help improve the ionic conductivity and bonding performance of the binder composition and improve the rate performance of the battery.
[0177] Comparing Example 1 with Example 2-5, the monomer content in the polymer is changed alone, wherein the amount of the monomer containing the nitroaniline group added is in the range of 10 to 30 parts, and the more the amount of the monomer containing the nitroaniline group added, the greater the ionic conductivity of the binder composition, and the better the rate performance of the battery. Comparing Example 1 with Example 6-9, the content of two monomers in the polymer is changed, wherein the more the monomer containing the nitroaniline group and the acrylic acid monomer are added, the greater the ionic conductivity of the binder composition, and the better the rate performance of the battery. Comparing Example 1 with Example 10-13, it is shown that the more the monomer containing the nitroaniline group and the acrylic acid monomer are added in the polymer, the higher the content of the acrylic acid ester monomer, the greater the ionic conductivity of the binder composition, the better the bonding, the higher the peel strength of the negative electrode sheet, the higher the cycle capacity retention rate, and the better the rate performance of the battery.
[0178] By comparing Examples 1-14 with Comparative Examples 1-10, it can be seen that by adding 30-50 parts of vinyl monomers, 30-50 parts of acrylic monomers, 10-30 parts of acrylate monomers, 10-30 parts of monomers containing nitroaniline groups, 0.5-3 parts of initiators, 0.1-5 parts of surfactants, and 100-200 parts of solvents to the polymer, the prepared binder composition has a high ionic conductivity, and the ionic conductivity is 7×10 -4 ~10×10 -4 S / cm range, the adhesion is good, and the peel strength of the prepared negative electrode sheet is greater than 11N / m, which helps to improve the cycle performance and rate performance of the battery.
[0179] Comparing Example 1 with Example 15, as long as the vinyl monomers, acrylic monomers, acrylate monomers, and monomers containing nitroaniline groups are within the scope defined in the present application, they all have the same effect, and all contribute to improving the ionic conductivity and bonding properties of the binder composition, improving the peel strength of the electrode, and improving the cycle performance and rate performance of the battery.
[0180] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A binder composition, characterized in that: The adhesive composition is obtained by reacting a raw material composition comprising a vinyl monomer, a (meth)acrylate monomer, a (meth)acrylic acid monomer, a nitroaniline-containing monomer, and an alkali metal compound; The weight ratio of the vinyl monomer, the (meth)acrylate monomer, the (meth)acrylic acid monomer, the nitroaniline-containing monomer and the alkali metal compound is 30-50:10-30:30-50:10-30:5-10; The vinyl monomer is selected from styrene; The (meth) acrylic monomer includes one or more of acrylic acid, methacrylic acid, ethacrylic acid, and propylacrylic acid; The acrylic acid ester monomers include one or more of ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, and sec-butyl acrylate; The monomer containing nitroaniline group includes one or more of 4-(3-nitroaniline)-4-oxy-2-butyric acid and N-(3-nitroanilino)acrylamide.
2. The adhesive composition according to claim 1, characterized in that The ionic conductivity of the binder composition is 7×10 -4 ~10×10 -4 S / cm.
3. A pole piece, characterized in that: The invention comprises a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material, a negative electrode conductive agent, a thickener and the binder composition according to any one of claims 1 to 2.
4. The pole piece according to claim 3, characterized in that: The peel strength of the pole piece is greater than 11 N / m.
5. A secondary battery, characterized in that: Including the pole piece as claimed in claim 3 or 4.