Method for evaluating calcium handling capacity of slag in VD degassing process of medium and low carbon aluminum killed steel
By calculating the reaction equilibrium constant between CaO and molten steel in medium and low carbon aluminum-killed steel, we evaluate the calcium processing ability of the slag, solve the problem of the impact of the reduction of CaO on the calcium content in medium and low carbon steel, and reduce the risk of large-sized Ds inclusions. Produced, improving the service life and production quality of steel.
Patent Information
- Application Number
- CN202410882263.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-03
AI Technical Summary
The existing technology lacks a method to evaluate the impact of the reduction of CaO in medium and low carbon steel on the calcium content in the steel. This results in the high frequency of large-sized Ds inclusions in medium and low carbon aluminum-killed steel, which affects the service life of the steel.
By obtaining the composition information of molten steel and slag, combined with the molecule-ion coexistence theory, Wagner equation and Van't Hoff's formula, the actual Gibbs free energy of the chemical reaction occurring at the steel slag interface is calculated to evaluate the calcium treatment capability of the slag. , determine the reaction equilibrium constant between CaO and molten steel, and then evaluate the ability of slag to transfer calcium to molten steel.
It effectively reduces the probability of large-sized Ds inclusions, reduces cracks at the interface with steel, increases the service life of medium and low carbon steel, provides a design solution for improving steel quality, and reduces production costs.
Smart Images

Figure CN118412053B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgical production, and in particular to a method for evaluating the calcium treatment capacity of slag in a VD degassing process of medium and low carbon aluminum killed steel. Background Art
[0002] Medium and low carbon aluminum killed steel represented by 42CrMo must have extremely high reliability due to its harsh service conditions. Large-sized inclusions in steel, especially low-melting-point CaO-MgO-Al2O3 inclusions (Ds inclusions), seriously harm the fatigue life of steel. Cracks will occur at the interface between the inclusions and the steel, causing the inclusions to become the source of fatigue failure. With the increasing requirements for the service life of steel, the control of large-sized Ds inclusions has become a common issue of concern to metallurgical workers.
[0003] VD degassing is a method of vacuum treatment of molten steel in which the primary molten steel of the LF furnace is placed in a closed tank and evacuated, while argon is blown and stirred at the bottom of the ladle. Pure molten steel is obtained through bottom argon blowing, stirring and vacuum degassing. VD degassing is a typical process for the generation of large-sized Ds inclusions. The reason is that a strong slag reaction occurs under high vacuum conditions, and the ability of the slag to transfer calcium to the molten steel, that is, the slag calcium processing capacity, is significantly increased compared to normal pressure. This part of calcium further reacts with the existing inclusions in the steel to form low-melting-point Ds inclusions containing calcium. Since the interfacial tension between the low-melting-point Ds inclusions and the molten steel is small, there is a high possibility that it will be inherited to the rolled product. Controlling the degree of slag reaction in the VD process and reducing the ability of the slag to transfer calcium to the molten steel are effective means to reduce the probability of large-sized Ds inclusions.
[0004] After searching, the paper "Thermodynamics and Influencing Factors Analysis of CaO in Carbon-Reduced Slag of Bearing Steel in VD Furnace" was found. This paper uses the Lupis-Wagner method to calculate the possibility of carbon reduction of CaO in slag during VD furnace smelting, and qualitatively evaluates the effects of vacuum, temperature, and slag basicity on the calcium content in steel caused by carbon reduction of CaO in slag. It is finally shown that in the VD furnace, the carbon in the bearing steel can reduce the CaO in the slag to generate [Ca], which combines with Al2O3 in the steel to form point-shaped calcium aluminate inclusions. This paper only qualitatively evaluates the effect of the reduction of CaO in high-carbon bearing steel on the calcium content in steel, and does not take into account the effect of the reduction of CaO in medium and low carbon steels on the calcium content in steel, and its application is relatively single.
[0005] The paper "Effect of VD Refining Process on Total Oxygen and [Al]s Content in GCr15 Steel" analyzes the effect of slag basicity on [Al]s in steel, as well as the effect of vacuum degree and vacuum time on total oxygen in steel. The paper also focuses on the effect of CaO reduction in GCr15 high carbon bearing steel on the calcium content in the steel, but does not consider the effect of CaO reduction in medium and low carbon steels.
[0006] In view of the impact of large-sized Ds inclusions on the service life of medium and low carbon aluminum killed steel, and the lack of consideration in the existing technology on the impact of CaO reduction in medium and low carbon steel on the calcium content in the steel, it is urgently necessary to develop a method to evaluate the ability of slag in medium and low carbon steel to transfer calcium to molten steel during the VD degassing process, and analyze the factors affecting the steel caused by the reduction of CaO in medium and low carbon steel, so as to reduce the probability of the occurrence of large-sized Ds inclusions.
[0007] The present invention provides a method for evaluating the calcium treatment capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel, so as to solve the problem in the prior art that there is a lack of a method for evaluating the influence of CaO reduction on the calcium content in steel during the production process of medium and low carbon steel, reduce the probability of occurrence of large-sized Ds inclusions, reduce cracks generated at the interface between large-sized Ds inclusions and steel, and improve the service life of medium and low carbon steel. Summary of the invention
[0008] The purpose of the present invention is to provide a method for evaluating the calcium treatment capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel, so as to solve the problem in the prior art that there is a lack of a method for evaluating the effect of CaO reduction on the calcium content in steel during the production process of medium and low carbon steel, reduce the generation of large-sized Ds inclusions, reduce the probability of large-sized Ds inclusions, and improve the service life of medium and low carbon steel.
[0009] The technical solution of the present invention is: a method for evaluating the calcium treatment capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel, comprising the following steps:
[0010] S1. Obtain the molten steel temperature, molten steel composition information and slag composition information when the VD enters the station;
[0011] S2, according to the molten steel temperature and slag component information obtained in step S1, combined with the molecular-ion slag coexistence theory, calculate the activity of each component in the slag;
[0012] S3, calculating the activity coefficient of Al in the molten steel according to the molten steel temperature and molten steel component information obtained in step S1 and in combination with the Wagner equation;
[0013] S4. Combined with the Van't Hoff formula, the actual Gibbs free energy of the chemical reaction occurring at the slag interface is calculated, and combined with the actual Gibbs free energy, the calcium handling capacity of the slag is evaluated.
[0014] Preferably, the calcium handling capacity of the slag is the ability of the slag to transfer calcium to molten steel.
[0015] Preferably, the obtained molten steel component information includes the contents of C, Si, Mn, P, S, Cr, Ti, and Al in the molten steel;
[0016] The obtained slag component information includes the contents of CaO, SiO2, MgO, and Al2O3 in the slag.
[0017] Preferably, at the steel-slag interface, Al in the molten steel reacts with CaO in the slag, and the reaction products are Al2O3 and Ca, and Ca is in a gaseous state; the reaction equation of the reaction is as follows:
[0018]
[0019] The actual Gibbs free energy of the reaction is calculated as:
[0020] (1)
[0021] The equilibrium constant of the reaction is calculated as:
[0022] (2)
[0023] In the formula, [] and () represent the components in the molten steel and the slag, respectively, (g) represents that the product Ca is in gaseous state, △G, is the actual Gibbs free energy and standard Gibbs free energy required for the reaction to occur, K is the equilibrium constant of the reaction, R is a constant of 8.314, T is the temperature of the molten steel, , , , is the activity of CaO, Ca(g), Al2O3, and Al, , are Ca partial pressure and standard atmospheric pressure 101325Pa, [%Al] is the mass fraction of Al element, is the activity coefficient of Al element in molten steel.
[0024] Preferably, when calculating the activities of CaO, SiO2, MgO and Al2O3 in the slag in combination with the molecule-ion coexistence theory, the structural units in the slag components include simple ions, simple molecules and complex molecules;
[0025] The structural units in the slag components exist continuously within the range of the components studied, and a dynamic equilibrium exists between the simple molecules and the ions;
[0026] The process of forming the complex molecular compound follows the law of conservation of mass, and the corresponding chemical reaction equilibrium constant can be expressed as a function of mass action concentration.
[0027] Preferably, the activity coefficient of Al in the molten steel is calculated by the following formula:
[0028] (3)
[0029] Wherein, %C, %Si, %Mn, %P, %S, %Cr, %Ti and %Al are the contents of C, Si, Mn, P, S, Cr, Ti and Al in the molten steel.
[0030] Preferably, by substituting the formulas (2) and (3) into the formula (1), the relationship between the actual Gibbs free energy of the reaction and the molten steel temperature, the molten steel composition and the slag composition can be obtained:
[0031] (4)
[0032] The actual Gibbs free energy of the reaction between Al in the molten steel and CaO in the slag can be calculated by the relation (4).
[0033] Compared with the prior art, the advantages of the present invention are:
[0034] (1) The present invention provides a method for evaluating the calcium handling capacity of slag in the VD degassing process of medium-low carbon aluminum killed steel. The method can be used to evaluate the effect of CaO reduction on the calcium content in the steel, especially to evaluate the calcium handling capacity of slag in the VD degassing process of medium-low carbon aluminum killed steel, solving the problem that there is a lack of a method for evaluating the effect of CaO reduction on the calcium content in the steel during the production process of medium-low carbon steel in the prior art. The evaluation method provided by the present invention evaluates the calcium handling capacity of the slag, that is, the ability of the slag to transfer calcium to the molten steel, by calculating the actual Gibbs free energy of the reaction between [Al] and (CaO) in the CaO-SiO2-Al2O3-MgO quaternary slag system corresponding to the equilibrium state of medium-low carbon aluminum killed steel under different conditions in the actual production process; it is helpful to clarify the design scheme of the slag composition and the molten steel composition range in the actual production process, and is conducive to tracing the increase of large-sized inclusions and cracks at the steel interface caused by steel-slag mismatch, which can point out the direction for improving steel quality and effectively reduce the production cost of steel.
[0035] (2) The present invention provides a method for evaluating the calcium treatment capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel. The method is based on the steel-slag thermodynamic equilibrium condition, combined with the molecule-ion coexistence theory, Wagner equation and Van't Hoff formula, and establishes a Gibbs free energy calculation model. The method can quantitatively evaluate the relationship between the composition of molten steel, the temperature of molten steel and the composition of slag and the ability of slag to transfer Ca to molten steel, which helps to identify problems in the production process and provide corresponding improvement directions, clarify the process design plan, and then realize high-clean production of the VD process, which is of great significance to the improvement of production quality of modern steel enterprises. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0037] Figure 1 It is a flow chart of the method for evaluating the calcium treatment capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel according to the present invention;
[0038] Figure 2 This is a distribution diagram of inclusions in steel after VD breaking in Example 1 of the present invention;
[0039] Figure 3 This is a distribution diagram of inclusions in steel after VD breaking in Example 2 of the present invention;
[0040] Figure 4 This is a distribution diagram of inclusions in steel after VD breaking in Example 5 of the present invention;
[0041] Figure 5 This is a distribution diagram of inclusions in the steel after VD breaking in Example 11 of the present invention; DETAILED DESCRIPTION
[0042] The present invention is further described in detail below in conjunction with specific embodiments:
[0043] The embodiments provided in the present invention are all for evaluating the calcium transfer capability of wind power steel 42CrMo from slag to molten steel in the VD degassing process.
[0044] A method for evaluating the calcium handling capacity of slag in the VD degassing process of medium and low carbon aluminum killed steels, such as Figure 1 As shown, the following steps are included:
[0045] S1. Under different vacuum conditions, obtain the temperature of the molten steel, the content of the molten steel component information and the slag component information when the VD enters the station; the obtained molten steel component information includes the content of C, Si, Mn, P, S, Cr, Ti, Al and other components in the molten steel; the obtained slag component information includes the content of CaO, SiO2, MgO, Al2O3 and other components in the slag.
[0046] S2. According to the contents of CaO, SiO2, MgO, Al2O3 and other components in the CaO-SiO2-Al2O3-MgO quaternary slag system of the slag obtained in step S1, combined with the molecular-ion coexistence theory, the activities of the components such as CaO, SiO2, MgO, Al2O3 and other components in the slag are calculated; specifically as follows:
[0047] 1) Structural units in slag components, including simple ions, simple molecules and complex molecules; simple ions include Ca 2+ Mg 2+ , Fe 2+ , O 2-etc. Simple molecules include Al2O3, SiO2, MgO, etc. Complex molecules include CaO·2Al2O3, 2MgO·SiO2, CaO·MgO·2SiO2, etc.;
[0048] 2) The structural units in the slag components exist continuously within the range of the components studied, and there is a dynamic balance between simple molecules and ions:
[0049]
[0050] 3) The process of forming complex molecular compounds follows the law of conservation of mass, and the corresponding chemical reaction equilibrium constant can be expressed as a function of mass action concentration; the calculation formula of the reaction equilibrium constant is as follows:
[0051] (5)
[0052] in, is the mass action concentration of CaO·Al2O3; is the mass action concentration of CaO; is the mass action concentration of Al2O3.
[0053] The molar numbers of CaO, MgO, SiO2, and Al2O3 components in 100g of slag are defined as a1, a2, a3, and a4, respectively. The molar number of each component is calculated as follows:
[0054] , , , ;
[0055] (6)
[0056] The mass action concentration of CaO, MgO, SiO2 and Al2O3 in the slag is expressed as: , , , .
[0057] According to the coexistence theory, the mass action concentration of each structural unit is defined as the equilibrium molar fraction:
[0058] (7)
[0059] n i ——The equilibrium molar number of each component in the slag;
[0060] ∑n i ——The total number of moles in the slag.
[0061] Free metal ions Mg in slag2+ and O 2- Remain independent and will not form MgO. Therefore, the effective concentration of MgO can be expressed as:
[0062] (8)
[0063] According to the phase diagram, the structural units, chemical reactions, Gibbs free energy and mass action concentration expressions in the CaO-SiO2-Al2O3-MgO quaternary slag system can be determined, as shown in Tables 1 and 2.
[0064] Table 1. Expressions of structural units, molar numbers and mass action concentrations in slag
[0065]
[0066] Table 2. Chemical reaction equations, standard Gibbs free energy and mass action expressions for each reaction
[0067]
[0068] As shown in Table 1 and Table 2, N1-N 22 are the mass action concentrations of 22 molecules in the CaO-SiO2-Al2O3-MgO quaternary slag system, k1-k 18 They are the chemical equilibrium constants of 18 complex molecular compounds in the CaO-SiO2-Al2O3-MgO quaternary slag system.
[0069] According to the law of conservation of mass, the sum of the mass action concentrations of all structural units is 1. Combining the structural units in the slag components, the molar number of each structural unit and the mass action concentration expression shown in Table 1, and the chemical reactions, Gibbs free energy and mass action concentration expression in the slag components shown in Table 2, the sum of the mass action concentrations of all structural units can be expressed as:
[0070] (8)
[0071] According to the law of conservation of mass and combined with the expressions in Table 1 and Table 2, the calculation method of the molar number of CaO, SiO2, MgO and Al2O3 in the slag is as follows:
[0072]
[0073]
[0074]
[0075]
[0076] in, They respectively refer to the sum of the molar numbers of CaO in all CaO-containing components, the sum of the molar numbers of Al2O3 in all Al2O3-containing components, the sum of the molar numbers of SiO2 in all SiO2-containing components, and the sum of the molar numbers of MgO in all MgO-containing components.
[0077] With the help of the above formula, N1, N2, N3, and N4 can be solved using the fsolve function in MATLAB.
[0078] The contents of the components such as CaO, SiO2, MgO, Al2O3, etc. respectively obtained in step S1 of Examples 1-20 are combined with the above-mentioned molecule-ion coexistence theory and the above-mentioned calculation method to calculate the activities of the components such as CaO, SiO2, MgO, Al2O3, etc. in the slag in each example; the activities of CaO, SiO2, MgO, Al2O3 are shown in Table 3.
[0079] Table 3. Content and activity of CaO, SiO2, MgO, Al2O3 in slag in Examples 1-20
[0080]
[0081] Examples 1-20 are the contents of C, Si, Mn, P, S, Cr, Ti, Al and other components in the molten steel, as well as the contents of CaO, SiO2, MgO, Al2O3 and other components in the slag, obtained under different vacuum degrees, molten steel temperatures, molten steel components, slag components and other conditions; as shown in Table 3, combined with the molecule-ion coexistence theory and the above-mentioned calculation method, the activities of CaO, SiO2, MgO, Al2O3 and other components in the slag under different conditions were calculated.
[0082] S3. According to the C, Si, Mn, P, S, Cr, Ti and Al contents in the molten steel obtained in step S1, the activity coefficient of the Al element in the molten steel is calculated in combination with the Wagner equation. The calculation formula is as follows;
[0083] (3)
[0084] In the formula, is the activity coefficient of Al element in molten steel, [%C], [%Si], [%Mn], [%P], [%S], [%Cr], [%Ti] and [%Al] are the contents of C, Si, Mn, P, S, Cr, Ti and Al in molten steel respectively.
[0085] The contents of the components such as C, Si, Mn, P, S, Cr, Ti, Al, etc. in the molten steel obtained in step S1 of Examples 1-20 were combined with the above-mentioned Wagner equation to calculate the activity coefficient of the Al element in the molten steel in each example; the activity coefficients of the Al element in the molten steel of Examples 1-20 are shown in Table 4.
[0086] Table 4. Contents of C, Si, Mn, P, S, Cr, Ti, Al in the molten steel in Examples 1-20 and the contents of each component such as C, Si, Mn, P, S, Cr, Ti, Al in the molten steel
[0087]
[0088] As shown in Table 4, in combination with the Wagner equation, the activity coefficients of the Al element in the molten steel in Examples 1-20 for obtaining the molten steel temperature, molten steel component information, and slag component information under different conditions were calculated respectively.
[0089] S4: Combined with the Van't Hoff formula, the actual Gibbs free energy of chemical reaction at the slag interface is calculated, and combined with the actual Gibbs free energy, the calcium handling capacity of the slag is evaluated.
[0090] During the VD process, various chemical reactions will occur at the steel-slag interface, mainly the reaction between Al in the molten steel and CaO in the slag. Since the solubility of Ca in the molten steel is very low and the vapor pressure is very high, when Al in the molten steel reacts with CaO in the slag, the reaction products are Al2O3 and gaseous Ca. The reaction equation is as follows:
[0091]
[0092] The actual Gibbs free energy of the reaction is calculated as:
[0093] (1)
[0094] The equilibrium constant of the reaction is calculated as:
[0095] (2)
[0096] In the formula, [] and () represent the components in the molten steel and the slag, respectively, (g) represents that the product Ca is in gaseous state, △G, is the actual Gibbs free energy and standard Gibbs free energy required for the reaction to occur, K is the equilibrium constant of the reaction, R is a constant of 8.314, T is the temperature of the molten steel, , , , is the activity of CaO, Ca(g), Al2O3, and Al, , They are Ca partial pressure and standard atmospheric pressure 101325Pa respectively.
[0097] Substituting calculation formula (2) and calculation formula (3) in step S3 into formula 1, the relationship between the actual Gibbs free energy of the reaction and the molten steel temperature, molten steel composition and slag composition can be obtained:
[0098] (4)
[0099] The relevant results of Examples 1-20 calculated in Steps S2 and S3 are respectively substituted into the relational expression (4) in Step S4, and the actual Gibbs free energies of Examples 1-20 can be obtained by calculation. The actual Gibbs free energies of Examples 1-20 are shown in Table 5.
[0100] Table 5. Activities, activity coefficients, and actual Gibbs free energies of Examples 1-20
[0101]
[0102] Embodiments 1-20 are the molten steel temperature, molten steel component information, and slag component information obtained under different vacuum conditions, as shown in Table 5. Substituting the results of steps S2 and S3 into S4 can respectively calculate the actual Gibbs free energy in the equilibrium state corresponding to the chemical reaction between Al in the molten steel component and CaO in the slag component at the slag interface in Embodiments 1-20, that is, the Gibbs free energy in the CaO-SiO2-Al2O3-MgO quaternary slag system under the equilibrium state corresponding to medium and low carbon aluminum killed steel under different conditions; the calcium transfer ability of the slag to the molten steel can be evaluated according to the size of the actual Gibbs free energy.
[0103] When △G<0, it indicates that the chemical reaction between Al in the molten steel component and CaO in the slag component is a spontaneous process, that is, the slag has a strong ability to transfer calcium to the molten steel, and the smaller △G is, the easier it is for the chemical reaction between Al in the molten steel component and CaO in the slag component to occur; when △G>0, it indicates that the chemical reaction between Al in the molten steel component and CaO in the slag component is a non-spontaneous process, and the chemical reaction between Al in the molten steel component and CaO in the slag component is not easy to occur.
[0104] When Al in the molten steel component reacts chemically with CaO in the slag component, inclusions such as low-melting-point Ds inclusions will be generated in the molten steel. Since the interfacial tension between these inclusions and the molten steel is small, they are very likely to be inherited to the rolled product. Cracks will occur between the interface of large-sized inclusions in the steel and the steel, thus affecting the service life of the steel.
[0105] As shown in Table 5, the actual Gibbs free energy obtained by calculating the temperature, composition and components of the molten steel obtained in Example 1 is -12385.04 J / mol, which is less than zero, indicating that the chemical reaction between Al in the molten steel component and CaO in the slag component is a spontaneous process, that is, a chemical reaction can occur between Al in the molten steel component and CaO in the slag component. When the molten steel after VD is broken under the conditions corresponding to Example 1 is obtained, a small amount of inclusions can be found in the steel, such as Figure 2 The actual Gibbs free energy of the molten steel temperature, molten steel component and molten steel component obtained in Example 2, Example 5 and Example 11 is calculated to be -23801.69 J / mol, -25557.43 J / mol and -4423.26 J / mol, respectively, indicating that in Example 2, Example 5 and Example 11, the chemical reaction between Al in the molten steel component and CaO in the slag component is a spontaneous process, and the chemical reaction in Example 2 and Example 5 is easier to occur than the chemical reaction in Example 11; similarly, Figure 3 , Figure 4 , Figure 5 As shown, the molten steel after VD was broken under the conditions corresponding to Example 2, Example 5 and Example 11 was obtained respectively, and it can be found that inclusions also appeared in the steel. Comparing the molten steel after VD was broken under the conditions corresponding to Example 1, Example 2, Example 5 and Example 11 respectively, it can be found that the molten steel after VD was broken under the conditions corresponding to Example 2 and Example 5 obtained has significantly more inclusions in the steel. It can be seen that when △G is smaller, the reaction between Al in the molten steel component and CaO in the slag component is easier to occur; after VD is broken, there are more inclusions in the molten steel.
[0106] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the scope of protection of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description, and it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention.
Claims
1. A method for evaluating the calcium handling capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel, characterized in that: The following steps are involved: S1. Obtaining the temperature of the molten steel, the composition information of the molten steel and the composition information of the slag when the VD enters the station; wherein the obtained molten steel composition information includes the content of C, Si, Mn, P, S, Cr, Ti and Al in the molten steel; the obtained slag composition information includes the content of CaO, SiO2, MgO and Al2O3 in the slag; S2, according to the steel liquid temperature and slag component information obtained in step S1, combined with the molecular-ion slag coexistence theory, calculate the activities of CaO, SiO2, MgO, and Al2O3 in the slag; the structural units in the slag components include simple ions, simple molecules, and complex molecules; the structural units in the slag components exist continuously within the scope of the studied components, and there is a dynamic equilibrium between the simple molecules and the ions; the process of forming the complex molecular compound follows the law of conservation of mass, and the corresponding chemical reaction equilibrium constant can be expressed as a function of mass action concentration; S3, calculating the activity coefficient of Al in the molten steel according to the molten steel temperature and molten steel component information obtained in step S1 and in combination with the Wagner equation; S4. Calculate the actual Gibbs free energy of the chemical reaction occurring at the slag interface in combination with the Van't Hoff formula, and evaluate the calcium handling capacity of the slag in combination with the actual Gibbs free energy; the chemical reaction is a reaction between Al in the molten steel and CaO in the slag; Wherein, at the steel-slag interface, Al in the molten steel reacts with CaO in the slag, and the reaction products are Al2O3 and Ca, and Ca is in gaseous state; the reaction equation of the reaction is as follows: 2[Al]+3(CaO)=(Al2O3)+3Ca(g); The actual Gibbs free energy of the reaction is calculated as: ΔG=ΔG θ +RTInK (1) The equilibrium constant of the reaction is calculated as: In the reaction equation, "(g)" indicates that the product Ca is in gaseous state; in the calculation formula, △G, △G θ is the actual Gibbs free energy and standard Gibbs free energy required for the reaction to occur, K is the equilibrium constant of the reaction, R is a constant of 8.314, T is the temperature of the molten steel, and a CaO 、a Ca(g) , a Al is the activity of CaO, Ca(g), Al2O3, Al, p Ca 、p θ are Ca partial pressure and standard atmospheric pressure 101325Pa, [%Al] is the mass fraction of Al element, f Al is the activity coefficient of Al element in molten steel.
2. The method for evaluating the calcium treatment capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel according to claim 1, characterized in that: The activity coefficient of Al in the molten steel is calculated by the following formula: f Al =0.091×[%C]+0.0056×[%Si]+0.012×[%Mn]+0.05×[%P]+0.03×[%S]+0.025×[%Cr]+0.07×[%Ti]+0.045×[%Al] (3) Wherein, %C, %Si, %Mn, %P, %S, %Cr, %Ti, %Al are the contents of C, Si, Mn, P, S, Cr, Ti, Al in the molten steel.
3. The method for evaluating the calcium treatment capacity of slag in the VD degassing process of medium and low carbon aluminum killed steel according to claim 2, characterized in that: Substituting the above formulas (2) and (3) into the above formula (1), the relationship between the actual Gibbs free energy of the reaction and the molten steel temperature, molten steel composition and slag composition can be obtained: The actual Gibbs free energy of the reaction between Al in the molten steel and CaO in the slag can be calculated by the relation (4).