Double glass fiber covered copper rectangular wire and its preparation process
By adopting a three-layer insulating structure and specific chemical composition and treatment methods of modified glass wire, the heat resistance and service life problems of double-glass wire-clad copper flat wire are solved, and higher wear resistance and insulation performance are achieved, and the coil is extended service life.
Patent Information
- Application Number
- CN202410579934.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-11
AI Technical Summary
The existing double-glass wire wrapped copper flat wire is easily damaged during use, has poor heat resistance, resulting in a short service life, and the bending and adhesion performance of the winding wire is poor, which can easily lead to cracking of the insulation layer and affect the stability of the coil.
Double glass wire wrapped copper flat wire with three-layer insulating structure, including inner copper flat wire, first insulating paint layer, two modified glass wire and outermost insulating paint layer. The modified glass wire consists of specific chemical composition and treatment method Prepare, enhance its wear resistance and insulation properties, and improve overall performance by optimizing wrap angle and insulating paint layer thickness.
It significantly improves the wear resistance and oxidation resistance of glass wire, enhances the heat resistance and service life of copper flat wire, and improves the insulation effect and safety, extending the service life of the coil.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of double-glass-fiber-covered copper flat wires and relates to a double-glass-fiber-covered copper flat wire and a preparation process thereof. Background Art
[0002] With the rapid development of the transformer industry, especially the fierce competition in the dry-type transformer industry, some dry-type transformer manufacturers have begun to develop low-cost coils. The method is: wrap a glass fiber layer around the conductor to make it have good insulation properties. However, a large amount of heat will be generated during its operation. If the silk-wrapped copper flat wire does not have good heat resistance, it will easily be damaged after a few uses, and its service life will be short.
[0003] In addition, the winding wire currently used generally adopts copper flat wire or mica tape wrapped copper flat wire wrapped with double layer of glass wire, and a layer of bonding paint is coated between each layer and on the surface to solve the insulation problem. It has the advantages of good corona resistance, strong overload capacity and high temperature resistance. It is widely used in electric welding machines, plasma cutting machines, voltage stabilizers, dry-type transformers and reactors of large generator sets.
[0004] However, the double-layer glass fibers of these structures all use a small pitch, that is, a 1-2° wrapping angle. When winding the coil, the bending and adhesion performance of the winding wire cannot meet the requirements. During use, the insulation layer is prone to cracking on the bending surface of the winding coil, which damages the coil and shortens its service life. At the same time, during the use of the double-glass-fiber-wrapped copper flat wire, the copper flat wire will heat up, resulting in the copper flat wire temperature being too high or the outside temperature being too low, making the copper flat wire temperature unstable and the temperature changing greatly. Such high and low temperatures will reduce the service life of the copper flat wire, and the glass fiber itself has poor wear resistance and a low service life, so a new double-glass-fiber-wrapped copper flat wire is needed. Summary of the invention
[0005] The object of the present invention is to provide a double glass-fiber covered copper rectangular wire and a preparation process thereof, which has the characteristics of good wear resistance.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A double glass-fiber covered copper flat wire, comprising an inner copper flat wire, the outer portion of the copper flat wire is firstly a first insulating varnish layer, then evenly wrapped with two layers of modified glass fibers in opposite directions, a second insulating varnish layer is coated between the two layers of modified glass fibers, and a third insulating varnish layer is coated on the outermost modified glass fibers.
[0008] The chemical composition of the modified glass filaments includes, by weight percentage: 50-65% silicon dioxide, 10-15% aluminum oxide, 2-5% silicon carbide, 3-5% molybdenum disulfide, 2-5% boron oxide, 3-5% magnesium oxide, 5-10% zinc oxide, 2-5% titanium dioxide, 2-3% calcium fluoride, and 1-2% dispersant;
[0009] The modified glass filament is prepared by the following steps:
[0010] The raw materials for preparing modified glass fibers are mixed according to weight percentage, melted at 1300-1400° C. for 0.5-1 h, and then formed into glass fibers by a wire drawing machine. After the formed glass fibers are cooled to room temperature, they are first kept in a drying furnace at 500-600° C. for 1-2 h, and then kept in a drying furnace at 600-700° C. for 2-3 h to obtain dried glass fibers;
[0011] The xanthan gum is dissolved in deionized water at 30-40°C to prepare a xanthan gum solution with a mass fraction of 2-3wt%, and the dried glass fibers are added and stirred thoroughly, and then heated at 80-100°C to completely evaporate the deionized water, and dried to obtain dry glass fibers. The silane coupling agent is then dissolved in a solution with a mass ratio of water to ethanol of 1:9, and the solution is ultrasonically treated for 20 minutes, and then the pH value of the solution is adjusted to 3.5-4.0 with 15% dilute hydrochloric acid, and mixed and stirred for 1-1.2 hours to prepare a silane coupling agent solution with a mass fraction of 10%, and the dried glass fibers are immersed in the silane coupling agent solution, ultrasonically treated at room temperature for 1-1.5 hours, and dried at 120-150°C for 2-2.5 hours to obtain modified glass fibers.
[0012] As a preferred technical solution of the present invention, the insulating paint layer material is epoxy resin paint.
[0013] As a preferred technical solution of the present invention, the dispersant is one of sodium polyacrylate or polyethylene glycol monoallyl ether.
[0014] As a preferred technical solution of the present invention, the silane coupling agent is one of γ-aminopropyltriethoxysilane, vinyltriethoxysilane or 3-(3-aminophenoxy)propyltrimethoxysilane.
[0015] As a preferred technical solution of the present invention, the diameter of the modified glass filaments is 20 to 80 μm.
[0016] A preparation process of a double glass-fiber covered copper rectangular wire comprises the following steps:
[0017] S1. Use TU2R oxygen-free copper rod, semi-finished products are produced by extrusion process;
[0018] S2. Put the bare copper flat wire into the wire drawing machine for wire drawing. The wire drawing oil temperature in the wire drawing machine is less than 40℃.
[0019] S3, transferring the drawn copper flat wire into an annealing furnace, and annealing it at a speed of 150 m / min in a nitrogen atmosphere, and controlling the annealing temperature at 400±20°C;
[0020] S4. Use a micro-grinding tool to perform surface treatment on the annealed copper flat wire, then apply an insulating paint layer on the surface of the annealed copper flat wire, and dry it at 60° C. for 20 hours by vacuum baking to obtain a first insulating paint layer;
[0021] S5, wrapping the modified glass filaments on the copper flat wire, applying an insulating paint layer on the surface of the modified glass filaments, and drying the filaments at 60° C. for 20 hours by vacuum baking to obtain a second insulating paint layer;
[0022] S6. Wrap another layer of modified glass fiber in the opposite direction, apply a layer of insulating paint on the surface of the modified glass fiber wrapped in the opposite direction, and dry it at 60°C for 20 hours by vacuum baking to obtain a third layer of insulating paint. After standing for 24 hours, the product double glass fiber covered copper rectangular wire is obtained.
[0023] As a preferred technical solution of the present invention, it is characterized in that the thickness of the first insulating paint layer is 0.015-0.020 mm, the thickness of the second insulating paint layer is 0.015-0.018 mm, and the thickness of the third insulating paint layer is 0.020-0.025 mm.
[0024] As a preferred technical solution of the present invention, it is characterized in that the wrapping angle of the modified glass filament is 20 to 30 degrees.
[0025] Beneficial effects of the present invention:
[0026] (1) In the present invention, the performance of the glass filament is further improved by adding silicon carbide and molybdenum disulfide. Silicon carbide has extremely high hardness and strength, plays a role of filling and reinforcing in the material, and can significantly improve the wear resistance of the material. At the same time, silicon carbide has excellent thermal stability and can maintain structural stability at high temperatures, so that the glass filament can still maintain good performance in a high temperature environment; molybdenum disulfide is also a commonly used solid lubricant and wear-resistant agent, which has high temperature stability and good lubrication performance, and is suitable for high temperature and high load working environments.
[0027] (2) The addition of silicon carbide further improves the mechanical strength of the glass filaments. It also has barrier properties, which can reduce the penetration of external substances such as moisture and oxygen into the glass filaments, which helps to improve the oxidation resistance of the glass filaments. Through the treatment of silane coupling agent and xanthan gum, the silane molecules can be firmly connected to the surface of the glass filaments to form a silicon oxide film with high hardness and wear resistance. At the same time, xanthan gum has good stability, which effectively improves the wear resistance of the glass filaments. Three layers of insulating paint are coated in the structure, which can increase the wear resistance of the copper flat wire and improve its service life. At the same time, the paint film can also provide a certain insulation effect and enhance the overall safety. DETAILED DESCRIPTION
[0028] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.
[0029] Example 1
[0030] Preparation of modified glass fibers:
[0031] According to weight percentage, 55% of silicon dioxide, 15% of aluminum oxide, 2% of silicon carbide, 3% of molybdenum disulfide, 2% of boron oxide, 3% of magnesium oxide, 10% of zinc oxide, 5% of titanium dioxide, 3% of calcium fluoride, and 2% of sodium polyacrylate are mixed, melted at 1300° C. for 1 hour, and then formed into glass fibers by a wire drawing machine. After the formed glass fibers are cooled to room temperature, they are first kept warm at 500° C. for 2 hours in a drying furnace, and then kept warm at 600° C. for 3 hours to obtain dried glass fibers;
[0032] Xanthan gum was dissolved in deionized water at 30°C to prepare a xanthan gum solution with a mass fraction of 2wt%, dried glass fibers were added and stirred thoroughly, and then the deionized water was completely evaporated at 80°C, and dried to obtain dried glass fibers. γ-aminopropyltriethoxysilane was dissolved in a solution with a mass ratio of water to ethanol of 1:9, and the solution was ultrasonically treated for 20 minutes, and then the pH of the solution was adjusted to 3.5 with 15% dilute hydrochloric acid, and mixed and stirred for 1 hour to prepare a γ-aminopropyltriethoxysilane solution with a mass fraction of 10%, and the dried glass fibers were immersed in the γ-aminopropyltriethoxysilane solution, ultrasonically treated at room temperature for 1.5 hours, and dried at 120°C for 2 hours to obtain modified glass fibers with a diameter of 20μm.
[0033] Preparation of double glass fiber covered copper rectangular wire:
[0034] S1. Use TU2R oxygen-free copper rod, semi-finished products are produced by extrusion process;
[0035] S2. Put the bare copper flat wire into the wire drawing machine for wire drawing. The wire drawing oil temperature in the wire drawing machine is 35℃.
[0036] S3, transferring the drawn copper flat wire into an annealing furnace, and annealing it at a speed of 150 m / min in a nitrogen atmosphere, and controlling the annealing temperature at 400° C.;
[0037] S4. Use a micro-grinding tool to perform surface treatment on the annealed copper flat wire, then apply epoxy resin paint on the surface of the annealed copper flat wire, and dry it at 60° C. for 20 hours by vacuum baking to obtain a first insulating paint layer with a thickness of 0.015 mm;
[0038] S5, wrapping the modified glass filaments on the copper flat wire at a wrapping angle of 20°, applying epoxy resin paint on the surface of the modified glass filaments, and drying them at 60° C. for 20 hours by vacuum baking to obtain a second insulating paint layer with a thickness of 0.015 mm;
[0039] S6. Wrap another layer of modified glass fiber in the opposite direction with a wrapping angle of 20°, apply epoxy resin paint on the surface of the modified glass fiber wrapped in the opposite direction, and dry it at 60°C by vacuum baking for 20 hours to obtain a third layer of insulating paint layer with a thickness of 0.020mm. After standing for 24 hours, the product double glass fiber covered copper rectangular wire is obtained.
[0040] Example 2
[0041] Preparation of modified glass fibers:
[0042] According to weight percentage, 53% of silicon dioxide, 15% of aluminum oxide, 3% of silicon carbide, 4% of molybdenum disulfide, 2% of boron oxide, 3% of magnesium oxide, 10% of zinc oxide, 5% of titanium dioxide, 3% of calcium fluoride, and 2% of sodium polyacrylate are mixed, melted at 1350° C. for 1 hour, and then formed into glass fibers by a wire drawing machine. After the formed glass fibers are cooled to room temperature, they are first kept warm at 550° C. for 1.5 hours in a drying furnace, and then kept warm at 650° C. for 2.5 hours to obtain dried glass fibers;
[0043] Xanthan gum was dissolved in deionized water at 35°C to prepare a xanthan gum solution with a mass fraction of 2.5wt%. The dried glass fibers were added and stirred thoroughly. The solution was heated at 90°C to completely evaporate the deionized water and dried to obtain dry glass fibers. Vinyltriethoxysilane was dissolved in a solution with a mass ratio of water to ethanol of 1:9. The solution was ultrasonically treated for 20 minutes and then the pH value of the solution was adjusted to 3.5 with 15% dilute hydrochloric acid. The solution was mixed and stirred for 1 hour to prepare a vinyltriethoxysilane solution with a mass fraction of 10%. The dried glass fibers were immersed in the vinyltriethoxysilane solution, ultrasonically treated at room temperature for 1.5 hours, and dried at 120°C for 2 hours to obtain modified glass fibers with a diameter of 50μm.
[0044] Preparation of double glass fiber covered copper rectangular wire:
[0045] S1. Use TU2R oxygen-free copper rod, semi-finished products are produced by extrusion process;
[0046] S2. Put the bare copper flat wire into the wire drawing machine for wire drawing. The temperature of the wire drawing oil in the wire drawing machine is 35°C.
[0047] S3, transferring the drawn copper flat wire into an annealing furnace, and annealing it at a speed of 150 m / min in a nitrogen atmosphere, and controlling the annealing temperature at 400° C.;
[0048] S4. Use a micro-grinding tool to perform surface treatment on the annealed copper flat wire, then apply epoxy resin paint on the surface of the annealed copper flat wire, and dry it at 60° C. for 20 hours by vacuum baking to obtain a first insulating paint layer with a thickness of 0.017 mm;
[0049] S5, wrapping the modified glass filaments on the copper flat wire at a wrapping angle of 25°, applying epoxy resin paint on the surface of the modified glass filaments, and drying them at 60° C. for 20 hours by vacuum baking to obtain a second insulating paint layer with a thickness of 0.017 mm;
[0050] S6. Wrap another layer of modified glass fiber in the opposite direction with a wrapping angle of 25°, apply epoxy resin paint on the surface of the modified glass fiber wrapped in the opposite direction, and dry it at 60°C by vacuum baking for 20 hours to obtain a third layer of insulating paint with a thickness of 0.022mm. After standing for 24 hours, the product double glass fiber covered copper rectangular wire is obtained.
[0051] Example 3
[0052] Preparation of modified glass fibers:
[0053] According to weight percentage, 50% of silicon dioxide, 15% of aluminum oxide, 5% of silicon carbide, 5% of molybdenum disulfide, 2% of boron oxide, 3% of magnesium oxide, 10% of zinc oxide, 5% of titanium dioxide, 3% of calcium fluoride, and 2% of sodium polyacrylate are mixed, melted at 1400° C. for 1 hour, and then formed into glass fibers by a wire drawing machine. After the formed glass fibers are cooled to room temperature, they are first kept warm at 600° C. for 1.5 hours in a drying furnace, and then kept warm at 700° C. for 2 hours to obtain dried glass fibers;
[0054] Xanthan gum was dissolved in deionized water at 40°C to prepare a xanthan gum solution with a mass fraction of 3wt%, and dried glass fibers were added and stirred thoroughly. The mixture was heated at 100°C to completely evaporate the deionized water and dried to obtain dry glass fibers. 3-(3-aminophenoxy)propyltrimethoxysilane was dissolved in a solution with a mass ratio of water to ethanol of 1:9, and the solution was ultrasonically treated for 20 minutes. The pH value of the solution was adjusted to 3.5 with 15% dilute hydrochloric acid, and mixed and stirred for 1 hour to prepare a 10% 3-(3-aminophenoxy)propyltrimethoxysilane solution. The dried glass fibers were immersed in the 3-(3-aminophenoxy)propyltrimethoxysilane solution, ultrasonically treated at room temperature for 1.5 hours, and dried at 120°C for 2 hours to obtain modified glass fibers with a diameter of 80μm.
[0055] Preparation of double glass fiber covered copper rectangular wire:
[0056] S1. Use TU2R oxygen-free copper rod, semi-finished products are produced by extrusion process;
[0057] S2. Put the bare copper flat wire into the wire drawing machine for wire drawing. The wire drawing oil temperature in the wire drawing machine is 35℃.
[0058] S3, transferring the drawn copper flat wire into an annealing furnace, and annealing it at a speed of 150 m / min in a nitrogen atmosphere, and controlling the annealing temperature at 400° C.;
[0059] S4. Use a micro-grinding tool to perform surface treatment on the annealed copper flat wire, then apply epoxy resin paint on the surface of the annealed copper flat wire, and dry it at 60° C. for 20 hours by vacuum baking to obtain a first insulating paint layer with a thickness of 0.020 mm;
[0060] S5, wrapping the modified glass filaments on the copper flat wire at a wrapping angle of 30°, applying epoxy resin paint on the surface of the modified glass filaments, and drying them at 60° C. for 20 hours by vacuum baking to obtain a second insulating paint layer with a thickness of 0.018 mm;
[0061] S6. Wrap another layer of modified glass fiber in the opposite direction with a wrapping angle of 30°, apply epoxy resin paint on the surface of the modified glass fiber wrapped in the opposite direction, and dry it at 60°C by vacuum baking for 20 hours to obtain a third layer of insulating paint with a thickness of 0.025mm. After standing for 24 hours, the product double glass fiber covered copper rectangular wire is obtained.
[0062] Comparative Example 1
[0063] The difference between Comparative Example 1 and Example 1 is that molybdenum disulfide is not added to the chemical composition of the modified glass fiber, which includes, by weight percentage, 55% silicon dioxide, 15% aluminum oxide, 2% silicon carbide, 2% boron oxide, 3% magnesium oxide, 10% zinc oxide, 5% titanium dioxide, 3% calcium fluoride, 2% sodium polyacrylate, and 3% ethanol mixture, and the other operations are the same.
[0064] Comparative Example 2
[0065] The difference between Comparative Example 2 and Example 1 is that silicon carbide is not added to the chemical composition of the modified glass fiber, which includes, by weight percentage: 55% silicon dioxide, 15% aluminum oxide, 3% molybdenum disulfide, 2% boron oxide, 3% magnesium oxide, 10% zinc oxide, 5% titanium dioxide, 3% calcium fluoride, 2% sodium polyacrylate, and 2% ethanol mixture, and the other operations are the same.
[0066] Comparative Example 3
[0067] The difference between Comparative Example 3 and Example 1 is that the glass fibers are not treated with a silane coupling agent, and the other operations are the same.
[0068] Comparative Example 4
[0069] The difference between Comparative Example 4 and Example 1 is that the glass fibers are not treated with xanthan gum, and the other operations are the same.
[0070] Abrasion resistance and elongation are measured according to GB / T 4074.3-2008 standard:
[0071] The test results are shown in the following table:
[0072] Wear resistance Elongation / % Example 1 21.63N 26 Example 2 22.18N 28 Example 3 23.21N 30 Comparative Example 1 20.55N 23 Comparative Example 2 20.34N 22 Comparative Example 3 20.10N 20 Comparative Example 4 20.16N 20
[0073] From the experimental results, it can be seen that the wear resistance and elongation values measured in Examples 1-3 are greater than the data in Comparative Examples 1-4, indicating that the embodiments can withstand greater forces. Therefore, the double glass fiber covered copper rectangular wire prepared by the present invention has better wear resistance.
[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A double glass fiber covered copper rectangular wire, It is characterized in that The double glass-fiber-covered copper flat wire comprises an inner copper flat wire, the outer portion of which is firstly a first insulating paint layer, then evenly wrapped with two layers of modified glass fibers in opposite directions, a second insulating paint layer is coated between the two layers of modified glass fibers, and a third insulating paint layer is coated on the outermost modified glass fibers. The chemical composition of the modified glass filaments includes, by weight percentage: 50-65% silicon dioxide, 10-15% aluminum oxide, 2-5% silicon carbide, 3-5% molybdenum disulfide, 2-5% boron oxide, 3-5% magnesium oxide, 5-10% zinc oxide, 2-5% titanium dioxide, 2-3% calcium fluoride, and 1-2% dispersant; The modified glass filament is prepared by the following steps: The raw materials for preparing modified glass fibers are mixed according to weight percentage, melted at 1300-1400° C. for 0.5-1 h, and then formed into glass fibers by a wire drawing machine. After the formed glass fibers are cooled to room temperature, they are first kept in a drying furnace at 500-600° C. for 1-2 h, and then kept in a drying furnace at 600-700° C. for 2-3 h to obtain dried glass fibers; The xanthan gum is dissolved in deionized water at 30-40°C to prepare a xanthan gum solution with a mass fraction of 2-3wt%, and the dried glass fibers are added and stirred thoroughly, and then heated at 80-100°C to completely evaporate the deionized water, and dried to obtain dry glass fibers. The silane coupling agent is then dissolved in a solution with a mass ratio of water to ethanol of 1:9, and the solution is ultrasonically treated for 20 minutes, and then the pH value of the solution is adjusted to 3.5-4.0 with 15% dilute hydrochloric acid, and mixed and stirred for 1-1.2 hours to prepare a silane coupling agent solution with a mass fraction of 10%, and the dried glass fibers are immersed in the silane coupling agent solution, ultrasonically treated at room temperature for 1-1.5 hours, and dried at 120-150°C for 2-2.5 hours to obtain modified glass fibers.
2. The double glass-fiber covered copper rectangular wire according to claim 1, It is characterized in that The insulating paint layer material is epoxy resin paint.
3. The double glass-fiber covered copper rectangular wire according to claim 1, It is characterized in that The dispersant is one of sodium polyacrylate or polyethylene glycol monoallyl ether.
4. The double glass-fiber covered copper rectangular wire according to claim 1, It is characterized in that The silane coupling agent is one of γ-aminopropyltriethoxysilane, vinyltriethoxysilane or 3-(3-aminophenoxy)propyltrimethoxysilane.
5. The double glass-fiber covered rectangular copper wire according to claim 1, It is characterized in that The diameter of the modified glass filament is 20 to 80 μm.
6. A process for preparing a double glass fiber covered copper rectangular wire according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1. Use TU2R oxygen-free copper rod, semi-finished products are produced by extrusion process; S2. Put the bare copper flat wire into the wire drawing machine for wire drawing. The wire drawing oil temperature in the wire drawing machine is less than 40℃. S3, transferring the drawn copper flat wire into an annealing furnace, and annealing it at a speed of 150 m / min in a nitrogen atmosphere, and controlling the annealing temperature at 400±20°C; S4. Use a micro-grinding tool to perform surface treatment on the annealed copper flat wire, then apply an insulating paint layer on the surface of the annealed copper flat wire, and dry it at 60° C. for 20 hours by vacuum baking to obtain a first insulating paint layer; S5, wrapping the modified glass filaments on the copper flat wire, applying an insulating paint layer on the surface of the modified glass filaments, and drying the filaments at 60° C. for 20 hours by vacuum baking to obtain a second insulating paint layer; S6. Wrap another layer of modified glass fiber in the opposite direction, apply a layer of insulating paint on the surface of the modified glass fiber wrapped in the opposite direction, and dry it at 60°C for 20 hours by vacuum baking to obtain a third layer of insulating paint. After standing for 24 hours, the product double glass fiber covered copper rectangular wire is obtained.
7. The preparation process of the double glass fiber covered copper rectangular wire according to claim 6, It is characterized in that The thickness of the first insulating paint layer is 0.015-0.020 mm, the thickness of the second insulating paint layer is 0.015-0.018 mm, and the thickness of the third insulating paint layer is 0.020-0.025 mm.
8. The preparation process of the double glass fiber covered copper rectangular wire according to claim 6, It is characterized in that The wrapping angle of the modified glass yarn is 20 to 30 degrees.