A modified polyurethane composite sealing material and its preparation method

By forming zirconium dioxide on hollow glass microbeads and clicking reaction between silane coupling agent and cysteine, a modified filler is formed, which solves the problem of insufficient thermal stability and flame retardant properties of polyurethane sealant, and improves the composite The material's pressure and high temperature resistance properties also reduce costs.

CN118440489BActive Publication Date: 2024-11-19ZHUHAI LING HANG ELECTRIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410539908.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-11-19
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

Polyurethane sealants have poor thermal stability, insufficient flame retardant properties and high cost, while poor compatibility with organic materials leads to reduced wear resistance, tensile bending strength and high temperature resistance.

Method used

Zirconium dioxide is generated on hollow glass microbeads, and click reaction is carried out through silane coupling agent and cysteine ​​to form a modified filler, improving its compatibility with the matrix, enhancing pressure and high temperature resistance, and reducing the temperature resistance. cost.

Benefits of technology

It significantly improves the pressure resistance and high temperature resistance of composite materials, reduces the cost of raw materials, and solves the problem of insufficient thermal stability and flame retardant properties of polyurethane sealants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004820756460000021
    Figure BDA0004820756460000021
  • Figure BDA0004820756460000041
    Figure BDA0004820756460000041
  • Figure BDA0004820756460000061
    Figure BDA0004820756460000061
Patent Text Reader

Abstract

The present invention relates to a modified polyurethane composite plugging material and a preparation method thereof, and belongs to the technical field of plugging materials. A modified polyurethane composite plugging material comprises component A and component B, wherein component A comprises: glycerol-propylene oxide polyether, modified filler, leveling agent, antioxidant and catalyst; component B comprises: MDI and HDI; the modified filler is a hollow glass microsphere filler semi-coated with zirconium dioxide containing amino, carboxyl and hydroxyl groups on the surface. The present invention generates zirconium dioxide on hollow glass microspheres to form a composite material, and modifies it with a silane coupling agent, adds cysteine ​​for click reaction, and forms a modified filler with multiple active groups. This method improves the compatibility of microspheres and zirconium dioxide in the matrix, reduces agglomeration, enhances the pressure resistance and high temperature resistance of the composite material, and reduces the cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plugging materials and relates to a modified polyurethane composite plugging material and a preparation method thereof. Background Art

[0002] Polyurethane sealant, whose main component is polyurethane resin, exhibits excellent adhesion and plasticity. It can fit tightly with the cable sheath to form a solid sealing layer, effectively preventing the leakage of the cable's internal materials. At the same time, the sealant is wear-resistant and corrosion-resistant, and can resist erosion and friction from the external environment to ensure the durability of the sealing effect. However, polyurethane sealants also have some shortcomings, such as poor thermal stability, insufficient flame retardancy, and relatively high prices.

[0003] On the other hand, hollow glass microspheres have a smooth surface and are micron-sized hollow glass microspheres. Their core chemical composition is borosilicate glass, and their structure is a hollow transparent sphere. They appear as white flowing powder with a particle size between 5 and 130 microns. Hollow glass microspheres have many characteristics such as low density, high strength, high temperature resistance, acid and alkali resistance, low thermal conductivity, electrical insulation, good fluidity and chemical stability. They are a multifunctional cutting-edge new material with cross-domain applications, especially in the field of plugging materials. However, hollow glass microspheres are an inorganic material. Due to their poor compatibility with organic materials, this directly leads to a significant reduction in the key properties of organic materials such as wear resistance, tensile bending strength, compressive strength and high temperature resistance. Summary of the invention

[0004] The object of the present invention is to provide a modified polyurethane composite plugging material and a preparation method thereof. The present invention generates zirconium dioxide on hollow glass microspheres to form a composite material, and modifies it with a silane coupling agent, and adds cysteine ​​for click reaction to form a modified filler with multiple active groups. This method improves the compatibility of microspheres and zirconium dioxide in the matrix, reduces agglomeration, enhances the pressure resistance and high temperature resistance of the composite material, and reduces the cost.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A modified polyurethane composite plugging material comprises a component A and a component B in a mass ratio of 1:1.

[0007] Component A includes the following components by weight:

[0008]

[0009] Component B includes the following components by weight:

[0010] MDI 70-80 parts

[0011] HDI 30-35 parts;

[0012] Wherein, the preparation method of the modified filler comprises the following steps:

[0013] S1, after mixing hollow glass microspheres, zirconium oxychloride octahydrate and deionized water, adding additives and ammonia water for hydrothermal reaction, cooling, centrifugation washing, and drying to obtain a composite filler;

[0014] S2, adding the composite filler and the silane coupling agent to anhydrous ethanol, stirring for reaction, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight, to obtain a prefabricated filler;

[0015] S3. After mixing the prefabricated filler and anhydrous ethanol, add cysteine ​​and a photoinitiator, stir and react under ultraviolet light, filter, take the solid and wash it with anhydrous ethanol, and vacuum dry it until constant weight to obtain a modified filler.

[0016] As a preferred technical solution of the present invention, the catalyst is prepared by mixing triethylenediamine and dibutyltin diacetate in a mass ratio of 3-5:1-1.2.

[0017] As a preferred technical solution of the present invention, the leveling agent is one or two of polydimethylsiloxane and polymethylalkylsiloxane.

[0018] As a preferred technical solution of the present invention, the antioxidant is one or more of p-phenylenediamine, diaryl secondary amine, thioether and phosphite.

[0019] As a preferred technical solution of the present invention, the foaming agent in all embodiments and comparative examples of the present invention is water.

[0020] As a preferred technical solution of the present invention, in step S1, the dosage ratio of the hollow glass microspheres, zirconium oxychloride octahydrate, deionized water, additives and ammonia water is 2.5-3.5g:4-4.5g:25-30mL:0.3-0.5mL:3-4mL; the concentration of the ammonia water is 28%; the use of the additives promotes the dispersibility of zirconium dioxide during generation, and the in-situ generated zirconium dioxide can toughen the hollow glass microspheres, reduce the brittleness of the hollow glass microspheres, and thereby improve the compressive strength and high temperature resistance of the plugging material.

[0021] As a preferred technical solution of the present invention, in step S1, the temperature of the hydrothermal reaction is 200-240°C and the time is 6-8h.

[0022] As a preferred technical solution of the present invention, the auxiliary agent is prepared by mixing methionine, ethylene glycol and potassium chloride in a mass ratio of 5:3:11-12.

[0023] As a preferred technical solution of the present invention, in step S2, the mass ratio of the anhydrous ethanol, the composite filler and the silane coupling agent is 100-120:5-8:15-20; the silane coupling agent is vinyltrimethoxysilane; and the stirring reaction is stirred at 60-70°C for 6-8h.

[0024] As a preferred technical solution of the present invention, in step S3, the mass ratio of the prefabricated filler, anhydrous ethanol, cysteine ​​and photoinitiator is 10-12:80-100:4-6:0.5-1; the stirring reaction time is 60-90min; and the photoinitiator is one or more of benzoin methyl ether, benzoin dimethyl ether and benzoin ethyl ether.

[0025] The invention discloses a method for preparing a modified polyurethane composite plugging material, which comprises the following steps:

[0026] Component A: Mix glycerol-propylene oxide polyether, modified filler, leveling agent, catalyst and antioxidant at 30-50°C for 60 minutes, cool, and vacuum discharge and package;

[0027] Component B: Mix MDI and HDI evenly at 60-70℃, and then discharge and package under vacuum.

[0028] Beneficial effects of the present invention:

[0029] The invention generates zirconium dioxide in situ on hollow glass microspheres, and the hollow glass microspheres are semi-coated with zirconium dioxide to form a composite material. The surface of the composite material is modified by a silane coupling agent to introduce unsaturated carbon-carbon double bonds. Then, cysteine ​​is added to carry out a click reaction to form a modified filler having amino, hydroxyl and carboxyl groups. The compatibility of the hollow glass microspheres and zirconium dioxide in a matrix is ​​significantly improved, and the agglomeration of zirconium dioxide is reduced. At the same time, the above-mentioned active groups are added, and a series of complex reactions can occur with isocyanate in the reaction system, so that the pressure resistance and high temperature resistance of the composite material are significantly improved, and the cost of raw materials is reduced. DETAILED DESCRIPTION

[0030] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0031] Example 1

[0032] A modified polyurethane composite plugging material comprises a component A and a component B in a mass ratio of 1:1, wherein the component A comprises the following components in parts by weight:

[0033]

[0034] Component B includes the following components by weight:

[0035] MDI 70 parts

[0036] HDI 30 parts;

[0037] The catalyst is prepared by mixing triethylenediamine and dibutyltin diacetate in a mass ratio of 3:1;

[0038] The leveling agent is polydimethylsiloxane;

[0039] The antioxidant is p-phenylenediamine;

[0040] The preparation method of the modified filler comprises the following steps:

[0041] S1. After mixing hollow glass microspheres, zirconium oxychloride octahydrate and deionized water, an auxiliary agent and ammonia water are added for hydrothermal reaction, cooled, centrifuged and washed, and dried to obtain a composite filler; wherein the amount ratio of the hollow glass microspheres, zirconium oxychloride octahydrate, deionized water, auxiliary agent and ammonia water is 2.5g:4g:25mL:0.3mL:3mL; the temperature of the hydrothermal reaction is 200°C and the time is 6h; the concentration of the ammonia water is 28%; the auxiliary agent is prepared by mixing methionine, ethylene glycol and potassium chloride in a mass ratio of 5:3:11;

[0042] S2, adding composite filler and silane coupling agent to anhydrous ethanol, stirring and reacting, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight, to obtain a prefabricated filler; wherein the mass ratio of the anhydrous ethanol, composite filler and silane coupling agent is 100:5:15; the silane coupling agent is vinyltrimethoxysilane; the stirring reaction is stirring at 60°C for 6h;

[0043] S3, after mixing the prefabricated filler and anhydrous ethanol, adding cysteine ​​and a photoinitiator, stirring the reaction under ultraviolet light, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight to obtain a modified filler; wherein the mass ratio of the prefabricated filler, anhydrous ethanol, cysteine ​​and photoinitiator is 10:80:4:0.5; the stirring reaction time is 60 minutes; the photoinitiator is benzoin methyl ether;

[0044] A method for preparing a modified polyurethane composite plugging material comprises the following steps:

[0045] Component A: Mix glycerol-propylene oxide polyether, modified filler, leveling agent, catalyst, water and antioxidant at 30°C for 60 minutes, cool, and vacuum discharge and package;

[0046] Component B: Mix MDI and HDI evenly at 60℃, and then discharge and package under vacuum.

[0047] Example 2

[0048] A modified polyurethane composite plugging material comprises a component A and a component B in a mass ratio of 1:1, wherein the component A comprises the following components in parts by weight:

[0049]

[0050] Component B includes the following components by weight:

[0051] MDI 73 parts

[0052] HDI 32 parts;

[0053] The catalyst is prepared by mixing triethylenediamine and dibutyltin diacetate in a mass ratio of 3.7:1.1;

[0054] The leveling agent is polydimethylsiloxane;

[0055] The antioxidant is p-phenylenediamine;

[0056] The preparation method of the modified filler comprises the following steps:

[0057] S1. After mixing hollow glass microspheres, zirconium oxychloride octahydrate and deionized water, an auxiliary agent and ammonia water are added for hydrothermal reaction, cooled, centrifuged and washed, and dried to obtain a composite filler; wherein the amount ratio of the hollow glass microspheres, zirconium oxychloride octahydrate, deionized water, auxiliary agent and ammonia water is 2.8g:4.2g:27mL:0.37mL:3.3mL; the temperature of the hydrothermal reaction is 213°C and the time is 7h; the concentration of the ammonia water is 28%; the auxiliary agent is prepared by mixing methionine, ethylene glycol and potassium chloride in a mass ratio of 5:3:11.3;

[0058] S2, adding composite filler and silane coupling agent to anhydrous ethanol, stirring and reacting, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight, to obtain a prefabricated filler; wherein the mass ratio of the anhydrous ethanol, composite filler and silane coupling agent is 107:6:17; the silane coupling agent is vinyltrimethoxysilane; the stirring reaction is stirring at 63°C for 7h;

[0059] S3, after mixing the prefabricated filler and anhydrous ethanol, adding cysteine ​​and a photoinitiator, stirring the reaction under ultraviolet light, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight to obtain a modified filler; wherein the mass ratio of the prefabricated filler, anhydrous ethanol, cysteine ​​and photoinitiator is 10.7:87:4.7:0.7; the stirring reaction time is 70 minutes; the photoinitiator is benzoin methyl ether;

[0060] A method for preparing a modified polyurethane composite plugging material comprises the following steps:

[0061] Component A: Mix glycerol-propylene oxide polyether, modified filler, leveling agent, catalyst, water and antioxidant at 37°C for 60 minutes, cool, and vacuum discharge and package;

[0062] Component B: Mix MDI and HDI evenly at 63°C, and then discharge and package under vacuum.

[0063] Example 3

[0064] A modified polyurethane composite plugging material comprises a component A and a component B in a mass ratio of 1:1, wherein the component A comprises the following components in parts by weight:

[0065]

[0066] Component B includes the following components by weight:

[0067] MDI 77 parts

[0068] HDI 33 parts;

[0069] The catalyst is prepared by mixing triethylenediamine and dibutyltin diacetate in a mass ratio of 4.3:1.1;

[0070] The leveling agent is polydimethylsiloxane;

[0071] The antioxidant is p-phenylenediamine;

[0072] The preparation method of the modified filler comprises the following steps:

[0073] S1. After mixing hollow glass microspheres, zirconium oxychloride octahydrate and deionized water, an auxiliary agent and ammonia water are added for hydrothermal reaction, cooled, centrifuged and washed, and dried to obtain a composite filler; wherein the amount ratio of the hollow glass microspheres, zirconium oxychloride octahydrate, deionized water, auxiliary agent and ammonia water is 3.2g:4.3g:28mL:0.43mL:3.7mL; the temperature of the hydrothermal reaction is 227°C and the time is 7.5h; the concentration of the ammonia water is 28%; the auxiliary agent is prepared by mixing methionine, ethylene glycol and potassium chloride in a mass ratio of 5:3:11.7;

[0074] S2, adding composite filler and silane coupling agent to anhydrous ethanol, stirring and reacting, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight, to obtain a prefabricated filler; wherein the mass ratio of the anhydrous ethanol, composite filler and silane coupling agent is 113:7:18; the silane coupling agent is vinyltrimethoxysilane; the stirring reaction is stirring at 67°C for 7.3h;

[0075] S3, after mixing the prefabricated filler and anhydrous ethanol, adding cysteine ​​and a photoinitiator, stirring the reaction under ultraviolet light, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight to obtain a modified filler; wherein the mass ratio of the prefabricated filler, anhydrous ethanol, cysteine ​​and photoinitiator is 11.3:93:5.3:0.8; the stirring reaction time is 80 minutes; the photoinitiator is benzoin methyl ether;

[0076] A method for preparing a modified polyurethane composite plugging material comprises the following steps:

[0077] Component A: Mix glycerol-propylene oxide polyether, modified filler, leveling agent, catalyst, water and antioxidant at 43°C for 60 minutes, cool, and vacuum discharge and package;

[0078] Component B: Mix MDI and HDI evenly at 67°C, and then discharge and package under vacuum.

[0079] Example 4

[0080] A modified polyurethane composite plugging material comprises a component A and a component B in a mass ratio of 1:1, wherein the component A comprises the following components in parts by weight:

[0081]

[0082]

[0083] Component B includes the following components by weight:

[0084] MDI 80 parts

[0085] HDI 35 parts;

[0086] The catalyst is prepared by mixing triethylenediamine and dibutyltin diacetate in a mass ratio of 5:1.2;

[0087] The leveling agent is polydimethylsiloxane;

[0088] The antioxidant is p-phenylenediamine;

[0089] The preparation method of the modified filler comprises the following steps:

[0090] S1. After mixing hollow glass microspheres, zirconium oxychloride octahydrate and deionized water, an auxiliary agent and ammonia water are added for hydrothermal reaction, cooled, centrifuged and washed, and dried to obtain a composite filler; wherein the amount ratio of the hollow glass microspheres, zirconium oxychloride octahydrate, deionized water, auxiliary agent and ammonia water is 3.5g:4.5g:30mL:0.5mL:4mL; the temperature of the hydrothermal reaction is 240°C and the time is 8h; the concentration of the ammonia water is 28%; the auxiliary agent is prepared by mixing methionine, ethylene glycol and potassium chloride in a mass ratio of 5:3:12;

[0091] S2, adding composite filler and silane coupling agent to anhydrous ethanol, stirring and reacting, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight, to obtain a prefabricated filler; wherein the mass ratio of the anhydrous ethanol, composite filler and silane coupling agent is 120:8:20; the silane coupling agent is vinyltrimethoxysilane; the stirring reaction is stirring at 70°C for 8h;

[0092] S3, after mixing the prefabricated filler and anhydrous ethanol, adding cysteine ​​and a photoinitiator, stirring the reaction under ultraviolet light, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight to obtain a modified filler; wherein the mass ratio of the prefabricated filler, anhydrous ethanol, cysteine ​​and photoinitiator is 12:100:6:1; the stirring reaction time is 90 minutes; the photoinitiator is benzoin methyl ether;

[0093] A method for preparing a modified polyurethane composite plugging material comprises the following steps:

[0094] Component A: Mix glycerol-propylene oxide polyether, modified filler, leveling agent, catalyst, water and antioxidant at 50°C for 60 minutes, cool, and vacuum discharge and package;

[0095] Component B: Mix MDI and HDI evenly at 70℃, and then discharge and package them in vacuum.

[0096] Comparative Example 1

[0097] Compared with Example 3, step S1 is not performed in comparative example 1, and the composite material in step S2 is prepared by mixing hollow glass microspheres and zirconium dioxide in a mass ratio of 3.2:4.3, and the remaining components, preparation steps and parameters are the same.

[0098] Comparative Example 2

[0099] Compared with Example 3, the difference is that Comparative Example 2 uses hollow glass microspheres instead of the composite filler in step S2, and the other components, preparation steps and parameters are the same.

[0100] Comparative Example 3

[0101] Compared with Example 3, the difference is that zirconium dioxide is used in Example 3 to replace the composite filler in step S2, and the other components, preparation steps and parameters are the same.

[0102] Comparative Example 4

[0103] Compared with Example 3, the difference is that no auxiliary agent is used in Comparative Example 4, and the other components, preparation steps and parameters are the same.

[0104] Comparative Example 5

[0105] Compared with Example 3, the difference is that in Example 5, step S3 is not performed, the prefabricated filler replaces the modified filler, and the other components, preparation steps and parameters are the same.

[0106] The components A and B of the plugging materials of Examples 1-4 and Comparative Examples 1-5 were mixed and cured to obtain finished products for the following tests:

[0107] Compression performance test: a universal testing machine was used to test the compression performance of the samples according to GB / T8813-2008. The sample size was 50mm×50mm×50mm, the uniform loading rate was 0.3mm / s, the compression strain was 10%, and 5 samples were tested in each group. The results were averaged.

[0108] High temperature resistance test: Aging for 48 hours in an oxidation box at 160°C, 80% humidity and 2 bar pressure, and then the above-mentioned pressure resistance test is performed after aging. The test results are shown in Table 1.

[0109] Table 1

[0110]

[0111] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-5, the pressure resistance and high temperature resistance of the modified polyurethane composite plugging material prepared in Examples 1-4 are significantly better than those in Comparative Examples 1-5.

[0112] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A modified polyurethane composite plugging material, It is characterized in that It includes component A and component B in a mass ratio of 1:

1. Component A includes the following components by weight: Component B includes the following components by weight: MDI 70-80 parts HDI 30-35 parts; Wherein, the preparation method of the modified filler comprises the following steps: S1, after mixing hollow glass microspheres, zirconium oxychloride octahydrate and deionized water, adding additives and ammonia water for hydrothermal reaction, cooling, centrifugation washing, and drying to obtain a composite filler; S2, adding the composite filler and the silane coupling agent to anhydrous ethanol, stirring for reaction, filtering, washing the solid with anhydrous ethanol, and vacuum drying until constant weight, to obtain a prefabricated filler; S3. After mixing the prefabricated filler and anhydrous ethanol, add cysteine ​​and a photoinitiator, stir and react under ultraviolet light, filter, take the solid and wash it with anhydrous ethanol, and vacuum dry it until constant weight to obtain a modified filler.

2. A modified polyurethane composite plugging material according to claim 1, Features: The catalyst is prepared by mixing triethylenediamine and dibutyltin diacetate in a mass ratio of 3-5:1-1.

2.

3. A modified polyurethane composite plugging material according to claim 1, Features: The leveling agent is one or two of polydimethylsiloxane and polymethylalkylsiloxane.

4. A modified polyurethane composite plugging material according to claim 1, Features: The antioxidant is one or more of p-phenylenediamine, diaryl secondary amine, thioether and phosphite.

5. The modified polyurethane composite plugging material according to claim 1, Features: In step S1, the usage ratio of the hollow glass microspheres, zirconium oxychloride octahydrate, deionized water, additives and ammonia water is 2.5-3.5 g: 4-4.5 g: 25-30 mL: 0.3-0.5 mL: 3-4 mL; the concentration of the ammonia water is 28%.

6. The modified polyurethane composite plugging material according to claim 1, Features: In step S1, the hydrothermal reaction temperature is 200-240° C. and the time is 6-8 hours.

7. The modified polyurethane composite plugging material according to claim 1, Features: The auxiliary agent is prepared by mixing methionine, ethylene glycol and potassium chloride in a mass ratio of 5:3:11-12.

8. The modified polyurethane composite plugging material according to claim 1, Features: In step S2, the mass ratio of the anhydrous ethanol, the composite filler and the silane coupling agent is 100-120:5-8:15-20; the silane coupling agent is vinyltrimethoxysilane; and the stirring reaction is carried out at 60-70° C. for 6-8 hours.

9. The modified polyurethane composite plugging material according to claim 1, Features: In step S3, the mass ratio of the prefabricated filler, anhydrous ethanol, cysteine ​​and photoinitiator is 10-12:80-100:4-6:0.5-1; the stirring reaction time is 60-90 minutes; and the photoinitiator is one or more of benzoin methyl ether, benzoin dimethyl ether and benzoin ethyl ether.

10. A method for preparing the modified polyurethane composite plugging material according to any one of claims 1 to 9, It is characterized in that The preparation method comprises the following steps: Component A: Mix glycerol-propylene oxide polyether, modified filler, leveling agent, catalyst and antioxidant at 30-50°C for 60 minutes, cool, and vacuum discharge and package; Component B: Mix MDI and HDI evenly at 60-70℃, and then discharge and package under vacuum.