Polyurethane elastomer composition, polyurethane elastomer composite material for labor protection shoe toe cap and preparation method thereof
Through the composite technology of polyurethane elastomer and fiber material, the problems of bulky toe and magnetic field detection of labor-protective shoes are solved, and the performance of lightweight, wear-resistant and flame-retardant is achieved, and the production process is simplified, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202410928399.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The existing labor-protective shoes and toe mainly rely on metal materials, which leads to bulky, inconvenient wear and unable to pass the magnetic field detection of airports and railway stations, and lacks efficient and environmentally friendly preparation technology.
The polyurethane elastomer composition is combined with fiber material, and the combination of low viscosity and high hardness polyurethane adhesive and fiber material is used to prepare a lightweight, wear-resistant and flame-retardant labor-protected shoe toe, and a simple process is used to realize large-scale industrialization. Production.
It realizes the high hardness, toughness and flame retardant properties of labor-protected shoes, while reducing specific gravity and thermal conductivity, improving wearable comfort and safety performance, and the process is environmentally friendly and pollution-free, suitable for large-scale production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane elastomers, and in particular relates to a polyurethane elastomer composition and a polyurethane elastomer composite material for labor insurance shoe toe caps and a preparation method thereof. Background Art
[0002] Labor protection shoes, also known as safety shoes or protective shoes, are a type of footwear that provides safety protection for the feet. Their main function is to prevent objects from hitting, stabbing or squeezing the instep and toes. At present, the protective function of labor protection shoes on the market is mainly achieved by metal toe caps. Generally, steel toe caps are made of 25, 40, 45 or 50 cold-rolled steel, or aluminum alloy toe caps with a slightly lower density are used. Metal labor protection shoes are safe and reliable, but they are bulky and inconvenient to wear. Metal toe caps cannot pass the magnetic field detection of airports and railway stations, affecting people's normal travel. Composite materials with lighter density and higher strength are used to make labor protection shoes. Toe caps made of composite materials have better air permeability and are more comfortable to wear. In addition, the low thermal conductivity and flame retardant properties of composite materials make them safer.
[0003] At present, there are few reports on the use of polyurethane to make labor protection shoe toe caps on the market. As a new type of high molecular polymer material, polyurethane is known as "liquid rubber". It has high wear resistance, high tear strength, high load-bearing capacity, and excellent low temperature resistance, oil resistance, aging resistance and other properties. Moreover, its raw materials are mostly liquid, and can be quickly formed without high temperature and high heat. The preparation process is simple, the operation is convenient, and the raw materials are environmentally friendly and pollution-free. The prepared labor protection shoe toe caps are more suitable for large-scale, large-scale, and low-cost production. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a polyurethane elastomer composition, which has low viscosity, does not need high temperature heating for preforming, has fast strength, high hardness, is lighter, has better toughness, flame retardant and wear-resistant properties, and is easier to make objects with high size requirements, different shapes and even special shapes. The present invention also provides a polyurethane elastomer composite material for labor insurance shoe toe caps and a preparation method thereof, which has a simple operation process and is easy to be mass-produced industrially.
[0005] The polyurethane elastomer composition of the present invention comprises component A and component B in a mass ratio of 100:(80-120):
[0006] Component A is composed of the following raw materials in percentage by mass:
[0007] Small molecule chain extender 5%-20%,
[0008] Flame retardant 10%-20%,
[0009] Combined polyether 31%-75%,
[0010] Modified Mannich polyether 5%-15%,
[0011] Coupling agent 0.5%-1%,
[0012] Defoaming agent 0-0.5%,
[0013] Water 0-0.1%,
[0014] Catalyst 0-0.05%,
[0015] Combined release agent 3.5%-5%,
[0016] Plasticizer 0-5%,
[0017] Combined antioxidant 1%-2.35%;
[0018] Component B is composed of the following raw materials in percentage by mass:
[0019] Polyether polyol 0-5%,
[0020] Isocyanate 85-100%,
[0021] Viscosity reducer 0-10%.
[0022] Preferably, the small molecule chain extender is one or more of dipropylene glycol, 1,2-propylene glycol, diethylene glycol, ethylene glycol, glycerol, and trimethylolpropane, with a number average molecular weight of 60-150 and a functionality of 2 or 3, more preferably 3.
[0023] Preferably, the flame retardant is one or two of triethyl phosphate, isopropylated triphenyl phosphate, diethyl ethyl phosphate, toluene diphenyl phosphate, tris(2-chloroethyl) phosphate, tris(2-chloropropyl) phosphate, preferably tris(chloropropyl) phosphate.
[0024] Preferably, the combined polyether is polyethylene oxide polyol or polypropylene oxide polyol, with a number average molecular weight of 375-3000, a functionality of 2, 3, or 4, and more preferably 3-4; the modified Mannich polyether is obtained by copolymerizing bisphenol A Mannich base and pentaerythritol initiator with ethylene oxide and propylene oxide, with an average hydroxyl value of 450 mgKOH / g and a functionality of 4.
[0025] Preferably, the coupling agent is one or more of KH-550, KH-560, KH-792, aniline propyl triethoxy silane, KH-590, and KH-570, and more preferably one or two of KH-560 and aniline propyl triethoxy silane.
[0026] Preferably, the combined mold release agent is a combination of an internal mold release agent and an external mold release agent, wherein the internal mold release agent is one or more of INT1948, 550D, and 8551, and the external mold release agent is a silicone mold release agent.
[0027] Preferably, the combined antioxidant is one or more combinations of an antioxidant, a light stabilizer, and a UV absorber, wherein the antioxidant is more preferably 1135, the light stabilizer is more preferably BASF5050, and the UV absorber is more preferably UV-1.
[0028] Preferably, in component B, the polyether polyol is polyoxypropylene polyol, with a number average molecular weight of 375-1000 and a functionality of 2 or 3.
[0029] Preferably, the isocyanate is one or more of diphenylmethane diisocyanate, carbodiimide-uretonimine modified MDI, and polymethylene polyphenyl isocyanate.
[0030] The polyurethane elastomer composite material for the toe cap of the labor protection shoe of the present invention is composited by fiber material and the polyurethane elastomer.
[0031] Preferably, the fiber material is alkali-free multi-axial glass fiber cloth or carbon fiber cloth.
[0032] The method for preparing the polyurethane elastomer composite material for the toe cap of the labor protection shoe of the present invention comprises the following steps:
[0033] (1) After mixing a small molecule chain extender, a flame retardant, a combined polyether, a modified Mannich polyether, a coupling agent, a defoamer, water, a catalyst, a combined mold release agent, a plasticizer, and a combined antioxidant, the mixture is fully stirred at 1000-1500 r / min using a high-speed disperser, and then packaged to obtain component A;
[0034] (2) reacting a polyether polyol having a moisture content of less than 0.05% with an isocyanate and a viscosity reducer at a temperature of 60-80°C for 2-3 hours to obtain a prepolymer having an isocyanate content of 26%-30.5%, and then vacuuming to remove mechanical bubbles and encapsulating to obtain component B;
[0035] (3) The mass ratio of component A, component B and fiber material is 100:(80-120):(220-410). Component A and component B are first mixed evenly in proportion and then impregnated into the fiber material laid in advance on the shoe toe mold. After reaching a gel state, compression molding is performed and the composite material is obtained after aging at 80-100° C. for 1-2 hours.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1. The present invention pre-lays the glass fiber skeleton and impregnates the polyurethane adhesive component to achieve the effect of bonding the glass fiber skeleton, so that the prepared labor protection shoe toe cap has high hardness and is lighter, has better toughness, and has flame retardant and wear-resistant properties. It is easier to manufacture objects with high size requirements, different shapes, and even special shapes, and is easy to polish and grind. The process is simple and easy to large-scale industrial production;
[0038] 2. The present invention introduces modified Mannich ethylene oxide / propane copolymer polyol, which has more aromatic ring structures and terminal hydroxyl active groups, has better compatibility with aromatic isocyanates such as MDI, and has its own self-catalytic effect, so that the system can reduce or even do not need to add additional catalysts to achieve rapid molding and demolding effects. The polyether initiator uses pentaerythritol, and its symmetrical structure makes the product have higher compressive strength, toughness and dimensional stability;
[0039] 3. In the present invention, a small amount of water can be added to component A to produce a high-hardness micro-foamed product, forming a micro-cavity structure on the basis of high load-bearing capacity, which has a lower thermal conductivity while being flame retardant, and the product quality is lighter;
[0040] 4. The present invention introduces a combination of internal and external release agents to make it easier to demould after the glass fiber is impregnated with polyurethane glue and solidified, without sticking to the mold, thereby reducing damage to the mold and increasing the service life of the mold;
[0041] 5. The manufacturing process of the present invention is simple, and it can be quickly solidified and formed without the need for preheating in the early forming stage. The raw materials used are safe, environmentally friendly and pollution-free, saving energy and resources. DETAILED DESCRIPTION
[0042] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.
[0043] Unless otherwise specified, all raw materials used in the examples are commercially available or prepared by existing methods. Unless otherwise specified, the percentages in the examples are by mass.
[0044] The materials used in the examples are as follows:
[0045] PPG400: number average molecular weight 400, functionality 2, hydroxyl value: 280±15 (mgKOH / g), polyoxypropylene glycol;
[0046] PPG1000: number average molecular weight 1000, functionality 2, hydroxyl value: 112±5 (mgKOH / g), polyoxypropylene glycol;
[0047] MN500: number average molecular weight 500, functionality 3, hydroxyl value: 340±10 (mgKOH / g), polyether polyol synthesized from propylene glycol and propylene oxide;
[0048] C304: number average molecular weight 375, functionality 3, hydroxyl value: 449±5 (mgKOH / g), polyether polyol synthesized from glycerol and propylene oxide;
[0049] NJ6209: Hydroxyl value: 380±15 (mgKOH / g) Polyether polyol synthesized from sorbitol and propylene oxide;
[0050] MN-3050: number average molecular weight 3000, functionality 3, hydroxyl value: 56±1.5 (mgKOH / g), polyoxypropylene triol;
[0051] MP-4450: homemade modified Mannich polyol, obtained by copolymerizing bisphenol A Mannich base and pentaerythritol initiator with ethylene oxide and propylene oxide, with a functionality of 4 and a hydroxyl value of 450±15 (mgKOH / g);
[0052] KG-03: molecular weight 93, functionality 3, purity 99.5% glycerol;
[0053] DPG: molecular weight 134, functionality 2, dipropylene glycol;
[0054] 103C: carbodiimide modified diphenylmethane diisocyanate;
[0055] PM200: polymethylene polyphenyl isocyanate;
[0056] DOTP: dioctyl terephthalate;
[0057] TXIB: 2,2,4-trimethyl-1,3-pentanediol diisobutyrate;
[0058] K-12: delayed tin catalyst;
[0059] Defoaming agent: X-203;
[0060] Flame retardants: tris(2-chloroethyl) phosphate (TCEP for short), tris(2-chloropropyl) phosphate (TCPP for short);
[0061] Coupling agent: KH-560, KH-792;
[0062] Internal release agent: 550D;
[0063] External release agent: silicone DY6012;
[0064] Combined antioxidant: 1135, BASF5050, UV-1;
[0065] Fiber material: E-glass fiber, Jushi Group Co., Ltd., 386T.
[0066] Example 1
[0067] The method for preparing the polyurethane elastomer composite material for the toe cap of the labor protection shoe comprises the following steps:
[0068] (1) 10% small molecule chain extender KG-03, 20% flame retardant TCPP, 53% polyether C304, 10% modified Mannich polyether MP-4450, 0.5% coupling agent KH-560, 0.1% defoamer X-203, 0.05% catalyst K-12, 3% internal release agent 550D, 1% external release agent DY6012, 2.35% combined antioxidant (1135: 0.7%, BASF5050: 0.5%, UV-1: 1.15%) were mixed, and then fully stirred at 1500r / min using a high-speed disperser, and then packaged to obtain component A;
[0069] (2) Component B is PM200, with an isocyanate content of 30.5%;
[0070] (3) The mass ratio of component A, component B and fiber material is 100:120:410. Component A and component B are first mixed evenly in proportion and then impregnated into the fiber material laid in advance on the shoe toe mold. After reaching a gel state, compression molding is performed and the composite material is obtained after aging at 80° C. for 2 hours.
[0071] Example 2
[0072] The method for preparing the polyurethane elastomer composite material for the toe cap of the labor protection shoe comprises the following steps:
[0073] (1) 20% small molecule chain extender DPG, 20% liquid flame retardant TCEP, 11% polyether MN500, 20.1% polyether NJ6209, 15% modified Mannich polyether MP-4450, 1% coupling agent KH-792, 0.5% defoamer X-203, 0.05% catalyst K-12, 3% internal release agent 550D, 2% external release agent DY6012, 2.35% combined antioxidant (1135: 0.7%, BASF5050: 0.5%, UV-1: 1.15%), and 5% plasticizer TXIB were mixed, and then fully stirred at 1000 r / min using a high-speed disperser and packaged to obtain component A;
[0074] (2) 3.3% of polyether polyol PPG1000 with a moisture content controlled below 0.05%, 10% of viscosity reducer DOTP and 86.7% of polyisocyanate PM200 were reacted at 75°C for 3 hours to obtain a prepolymer with an isocyanate content of 26%. The prepolymer was vacuumed to remove mechanical bubbles and then packaged to obtain component B;
[0075] (3) The mass ratio of component A, component B and fiber material is 100:100:245. Component A and component B are first mixed evenly in proportion and then impregnated into the fiber material laid in advance on the shoe toe mold. After reaching a gel state, compression molding is performed and the composite material is obtained after aging at 80° C. for 2 h.
[0076] Example 3
[0077] The method for preparing the polyurethane elastomer composite material for the toe cap of the labor protection shoe comprises the following steps:
[0078] (1) 5% small molecule chain extender KG-03, 10% liquid flame retardant TCEP, 20% polyether C304, 40% polyether NJ6209, 14% polyether MN-3050, 5% modified Mannich polyether MP-4450, 0.5% coupling agent KH-792, 0.1% water, 3% internal release agent 550D, 0.5% external release agent DY6012, 1.9% combined antioxidant (1135: 0.7%, BASF5050: 0.5%, UV-1: 0.7%) were mixed, and then fully stirred at 1500r / min using a high-speed disperser and packaged to obtain component A;
[0079] (2) 5% of polyether polyol MN500 with a moisture content controlled below 0.05%, 84.5% of polyisocyanate PM200, and 10.5% of isocyanate 103C are reacted at 80°C for 2h to obtain a prepolymer with an isocyanate content of 27.5%, which is then vacuumed to remove mechanical bubbles and then packaged to obtain component B;
[0080] (3) The mass ratio of component A, component B and fiber material is 100:100:371. Component A and component B are first mixed evenly in proportion and then impregnated into the fiber material laid in advance on the shoe toe mold. After reaching a gel state, compression molding is performed and the composite material is obtained after aging at 100° C. for 1 hour.
[0081] Example 4
[0082] The method for preparing the polyurethane elastomer composite material for the toe cap of the labor protection shoe comprises the following steps:
[0083] (1) 5% small molecule chain extender KG-03, 20% liquid flame retardant TCEP, 32% polyether NJ6209, 15% modified Mannich polyether MP-4450, 15% polyether MN-3050, 1% coupling agent KH-792, 0.5% defoamer X-203, 0.02% catalyst K-12, 4% internal release agent 550D, 1% external release agent DY6012, 1.48% combined antioxidant (1135: 0.5%, BASF5050: 0.3%, UV-1: 0.68%), and 5% plasticizer TXIB were mixed, and then fully stirred at 1500r / min using a high-speed disperser and packaged to obtain component A;
[0084] (2) 3% of polyether polyol PPG400 with a moisture content controlled below 0.05%, 93% of polyisocyanate PM200, and 4% of viscosity reducer DOTP were reacted at 80°C for 2 hours to obtain a prepolymer with an isocyanate content of 27.5%, and the prepolymer was vacuumed to remove mechanical bubbles and then packaged to obtain component B;
[0085] (3) The mass ratio of component A, component B and fiber material is 100:80:220. Component A and component B are first mixed evenly in proportion and then impregnated into the fiber material laid in advance on the shoe toe mold. After reaching a gel state, compression molding is performed and the composite material is obtained after aging at 100° C. for 1 hour.
[0086] Comparative Example:
[0087] Examples 1-3 in Chinese invention patent CN109371300B are used as comparative examples 1-3 of the present invention respectively;
[0088] The difference between Comparative Example 4 and Example 2 is that the modified Mannich polyether MP-4450 is not added, and the mass percentage of NJ6209 polyether is 35.1%;
[0089] The difference between Comparative Example 5 and Example 2 is that the modified Mannich polyether MP-4450 is replaced by the Mannich polyether of equal quality prepared by using the common initiator glycerol obtained in Example 2 of Chinese invention patent CN110591071B.
[0090] The performance tests of the polyurethane elastomer composite materials for labor protection shoe toe caps prepared in Examples 1-4 and Comparative Examples 1-5 are shown in Table 1.
[0091] Table 1 Performance test table of Examples 1-4 and Comparative Examples 1-5
[0092]
[0093] It can be seen from the above Examples 1-4 that the labor protection shoe toe caps made of the polyurethane elastomer composite material have lower specific gravity, higher strength, lower thermal conductivity, and higher safety performance; compared with Example 2 and Comparative Example 4 and Comparative Example 5, after the modified Mannich polyether of the present invention is added to the system, the high-temperature hardness of the system is higher and the deformation is smaller; compared with Examples 1-4 and Comparative Examples 1-3, the labor protection shoe toe caps of the present invention have greater advantages than metal toe caps, which have a thermal conductivity significantly lower than that of metal and are easier to mass produce.
Claims
1. A polyurethane elastomer composition, It is characterized in that It includes component A and component B with a mass ratio of 100: (80-120): Component A is composed of the following raw materials in percentage by mass: Small molecule chain extender 5%-20%, Flame retardant 10%-20%, Combined polyether 31%-75%, Modified Mannich polyether 5%-15%, Coupling agent 0.5%-1%, Defoaming agent 0-0.5%, Water 0-0.1%, Catalyst 0-0.05%, Combined release agent 3.5%-5%, Plasticizer 0-5%, Combined antioxidant 1%-2.35%; Component B is composed of the following raw materials in percentage by mass: Polyether polyol 0-5%, Isocyanate 85-100%, Viscosity reducer 0-10%; The modified Mannich polyether is obtained by copolymerizing bisphenol A Mannich base and pentaerythritol initiator with ethylene oxide and propylene oxide, with an average hydroxyl value of 450 mgKOH / g and a functionality of 4.
2. The polyurethane elastomer composition according to claim 1, It is characterized in that The small molecule chain extender is one or more of dipropylene glycol, 1,2-propylene glycol, diethylene glycol, ethylene glycol, glycerol, and trimethylolpropane, with a number average molecular weight of 60-150 and a functionality of 2 or 3.
3. The polyurethane elastomer composition according to claim 1, It is characterized in that The flame retardant is one or two of triethyl phosphate, isopropylated triphenyl phosphate, diethyl ethyl phosphate, toluene diphenyl phosphate, tri(2-chloroethyl) phosphate and tri(2-chloropropyl) phosphate.
4. The polyurethane elastomer composition according to claim 1, It is characterized in that The combined polyether is polyoxyethylene polyol or polyoxypropylene polyol, with a number average molecular weight of 375-3000 and a functionality of 2, 3 or 4.
5. The polyurethane elastomer composition according to claim 1, It is characterized in that The combined mold release agent is a combination of an internal mold release agent and an external mold release agent, wherein the internal mold release agent is one or more of INT1948, 550D, and 8551, and the external mold release agent is a silicone mold release agent.
6. The polyurethane elastomer composition according to claim 1, It is characterized in that The combined antioxidant is one or more combinations of an anti-aging agent, a light stabilizer, and an ultraviolet absorber.
7. The polyurethane elastomer composition according to claim 1, It is characterized in that In component B, the polyether polyol is polyoxypropylene polyol with a number average molecular weight of 375-1000 and a functionality of 2 or 3.
8. A polyurethane elastomer composite material for labor protection shoe toe caps, It is characterized in that It is made by compounding fiber material with the polyurethane elastomer described in any one of claims 1 to 7.
9. The polyurethane elastomer composite material for labor protection shoe toe caps according to claim 8, It is characterized in that The fiber material is alkali-free multi-axial glass fiber cloth or carbon fiber cloth.
10. A method for preparing the polyurethane elastomer composite material for labor protection shoe toe caps according to claim 8, It is characterized in that The steps include: (1) After mixing a small molecule chain extender, a flame retardant, a combined polyether, a modified Mannich polyether, a coupling agent, a defoamer, water, a catalyst, a combined mold release agent, a plasticizer, and a combined antioxidant, the mixture is fully stirred at 1000-1500 r / min using a high-speed disperser, and then packaged to obtain component A; (2) reacting a polyether polyol having a moisture content of less than 0.05% with an isocyanate and a viscosity reducer at a temperature of 60-80°C for 2-3 hours to obtain a prepolymer having an isocyanate content of 26%-30.5%, and then vacuuming to remove mechanical bubbles and encapsulating to obtain component B; (3) The mass ratio of component A, component B and fiber material is 100: (80-120): (220-410). Component A and component B are first mixed evenly in proportion and then impregnated into the fiber material laid on the shoe toe mold in advance. After reaching a gel state, compression molding is performed and the product is obtained after being aged at 80-100°C for 1-2 hours.
Citation Information
Cited By
Polyurethane elastomer composite material and production process thereof
CN122127574A